A rod-shaped ultrafine silver powder and its preparation method and application

By reacting silver source with reducing agent in the presence of ammonia water, and contact reaction between guide agent and capping agent in the presence of dispersant, rod-shaped ultrafine silver powder is prepared, and the silver powder has large particle size and dispersion in the prior art. The poor performance problem realizes the ability to form high-density circuits at low temperatures.

CN116213746BActive Publication Date: 2024-12-03HEBEI GUANGXING SEMICON TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310095144.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-10
Publication Date
2024-12-03
Estimated Expiration
2043-02-10

AI Technical Summary

Technical Problem

In the prior art, silver powder has a large average particle size, poor dispersion and high impurity content, making it difficult to form high-density and solid joints at low temperatures, and is not suitable for forming fine-pitch circuits.

Method used

By conducting a first contact reaction of the silver source with the reducing agent in the presence of ammonia, and then performing a second and third contact reaction in the presence of a dispersant, the reaction conditions such as temperature and time are controlled. and pressure to prepare rod-shaped ultrafine silver powder.

Benefits of technology

The average particle size and particle size distribution of silver powder are significantly reduced, its monodispersity and purity are improved, dense joints can be formed at low temperatures, and impurity content is reduced, and it is suitable for high-precision and high-density circuit formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116213746B_ABST
    Figure CN116213746B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of metallic silver nanomaterials, and discloses a rod-shaped ultrafine silver powder and a preparation method and application thereof. The method comprises: (1) in the presence of ammonia water, a silver source and a reducing agent are subjected to a first contact reaction to obtain a mixed solution I; (2) in the presence of a dispersant, the mixed solution I, a guiding agent and a capping agent are subjected to a second contact reaction and a third contact reaction in sequence. The average particle size of the ultrafine silver powder prepared by the method provided by the present invention is significantly reduced, and can be close to a monodisperse ultrafine silver powder, and the impurity content in the ultrafine silver powder can also be significantly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallic silver nanomaterials, and in particular to a rod-shaped ultrafine silver powder and a preparation method and application thereof. Background Art

[0002] The electrodes and circuits of emerging electronic and electrical devices such as HJT heterojunction solar cells, touch screen displays and infrared discharge detectors are all made by printing and sintering low-temperature conductive silver paste. As the demand for improving the performance potential of these electronic and electrical devices continues to increase, the electrodes and circuits are required to be significantly thinner, with higher wiring density and higher precision.

[0003] On the other hand, in the printed circuit forming process using low-temperature silver paste, the heating sintering temperature must be lower than 300°C or even lower, as low as 100°C, and excellent sintering performance must be obtained at low temperatures. The above performance requirements are a considerable technical challenge for the manufacture of ultra-fine silver powder for low-temperature silver paste.

[0004] Obviously, high fineness, high precision and lower sintering temperature requirements all require ultrafine silver powder with smaller particle size and better monodispersity.

[0005] At present, the average particle size of ultrafine silver powder produced by domestic silver powder manufacturers is about ≤0.5μm, and the particle size dispersion is very poor, which is far from the average particle size of silver powder ≤0.2μm and monodispersity required by advanced processes, and is not suitable for forming fine-pitch circuits. For these reasons, the market needs finer silver powder than ever before, whose dispersion is closer to monodispersity, less agglomeration of powder particles, and excellent low-temperature sintering properties.

[0006] At the same time, achieving dense and strong joints sintered at low temperatures (<200°C) remains a big challenge. The minimum sintering temperature strongly depends on the particle shape, particle spacing and surface energy. In this regard, rod-shaped silver powder has an advantage over spherical silver powder: the rod-shaped silver powder has a higher proportion of surface atoms and the ability to assemble into denser 3D colloids. Summary of the invention

[0007] The purpose of the present invention is to solve the problems in the prior art that the silver powder has a large average particle size, poor dispersibility and high impurity content.

[0008] In order to achieve the above object, the first aspect of the present invention provides a method for preparing rod-shaped ultrafine silver powder, the method comprising:

[0009] (1) in the presence of aqueous ammonia, subjecting a silver source and a reducing agent to a first contact reaction to obtain a mixed solution I;

[0010] (2) in the presence of a dispersant, subjecting the mixed solution I, the directing agent and the capping agent to a second contact reaction and a third contact reaction in sequence;

[0011] Wherein, in step (1), the reducing agent is a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.01-0.2:1; the concentration of the silver source in terms of silver ions is 0.01-0.5 mol / L, and the concentration of the reducing agent is 0.02-0.4 mol / L;

[0012] In step (2), the capping agent is a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 0.5-5:1.

[0013] Preferably, in step (1), the reducing agent is a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.02-0.05:1.

[0014] Preferably, in step (1), the concentration of the silver source in terms of silver ions is 0.05-0.2 mol / L, and the concentration of the reducing agent is 0.05-0.2 mol / L.

[0015] Preferably, in step (1), the conditions of the first contact reaction include at least: a temperature of 30-70° C. and a time of 30-60 min.

[0016] Preferably, in step (2), the directing agent is an aqueous solution of sodium sulfide and / or an aqueous solution of sodium hydrosulfide.

[0017] Preferably, in step (2), the molar ratio of the silver source calculated as silver ions to the directing agent calculated as dry basis is 1:0.001-0.01.

[0018] Preferably, in step (2), the capping agent is a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 2.3-3.6:1.

[0019] Preferably, in step (2), the number average molecular weight of the polyvinyl pyrrolidone is not greater than 15,000.

[0020] Preferably, in step (2), the conditions of the second contact reaction include at least: a temperature of 50-80° C. and a time of 30-60 min.

[0021] Preferably, in step (2), the conditions of the third contact reaction include at least: temperature of 60-100° C., pressure of 0.3-0.6 MPa, and time of 50-100 min.

[0022] The second aspect of the present invention provides rod-shaped ultrafine silver powder prepared by the method described in the first aspect.

[0023] The third aspect of the present invention provides the use of the rod-shaped ultrafine silver powder described in the second aspect in preparing a conductive silver paste.

[0024] The ultrafine silver powder prepared by the method provided by the present invention has a significantly reduced average particle size and a narrow particle size distribution, which can be close to monodisperse ultrafine silver powder, and can also significantly reduce the impurity content in the ultrafine silver powder; in particular, the average particle size of the ultrafine silver powder is reduced to below 0.3 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a scanning electron microscope characterization image of the rod-shaped ultrafine silver powder prepared in Example 1 of the present invention;

[0026] Figure 2 This is an X-ray diffraction characterization diagram of the rod-shaped ultrafine silver powder prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0028] In the present invention, unless otherwise specified, the room temperature or normal temperature refers to 25±2°C.

[0029] In the present invention, unless otherwise stated, the pressures described are gauge pressures.

[0030] As mentioned above, the first aspect of the present invention provides a method for preparing rod-shaped ultrafine silver powder, the method comprising:

[0031] (1) in the presence of aqueous ammonia, subjecting a silver source and a reducing agent to a first contact reaction to obtain a mixed solution I;

[0032] (2) in the presence of a dispersant, subjecting the mixed solution I, the directing agent and the capping agent to a second contact reaction and a third contact reaction in sequence;

[0033] Wherein, in step (1), the reducing agent is a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.01-0.2:1; the concentration of the silver source in terms of silver ions is 0.01-0.5 mol / L, and the concentration of the reducing agent is 0.02-0.4 mol / L;

[0034] In step (2), the capping agent is a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 0.5-5:1.

[0035] It should be noted that the reducing agent in the present invention is a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.01-0.2:1, that is, the reducing agent is a mixture. The concentration of the reducing agent represents the ratio of the total molar amount of hydrazine hydrate and ethylene glycol to the total volume of the reducing agent.

[0036] Preferably, in step (1), the reducing agent is a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.02-0.05:1. In the present invention, hydrazine hydrate has high reducing properties, which is conducive to quickly obtaining the seed body for the growth of silver particles; while ethylene glycol has a lower reducing property than hydrazine hydrate and a slower reaction rate. This slow reaction is conducive to controlling the shape of silver particles and may promote the generation of high-yield and monodisperse silver particles. However, the inventors have found that compounding hydrazine hydrate and ethylene glycol in a molar ratio of 0.02-0.05:1, combined with the other technical features of the technical solution provided by the present invention, can better control the shape of silver particles and obtain ultrafine silver powder with better dispersibility.

[0037] Preferably, in step (1), the concentration of the silver source in terms of silver ions is 0.05-0.2 mol / L, and the concentration of the reducing agent is 0.05-0.2 mol / L. In the present invention, as the concentration of silver ions increases, a higher amount of ultrafine silver powder can be obtained. If the concentration of silver ions is too high, the precipitated silver particles tend to agglomerate into very coarse particles, the particle size is no different from that of traditional silver powder, and the monodispersity is poor. When the concentration of silver ions is too low, the average particle size of the ultrafine silver powder is too small, the oil absorption increases, and the viscosity of the silver paste increases. However, the inventors have found that by controlling the concentration of the silver source in terms of silver ions in the range of 0.05-0.2 mol / L and the concentration of the reducing agent in the range of 0.05-0.2 mol / L, combined with the other technical features of the technical solution provided by the present invention, the yield of ultrafine silver powder can be higher and the monodispersity is better.

[0038] According to a particularly preferred embodiment of the present invention, in step (1), the silver source is silver nitrate.

[0039] Preferably, in step (1), the molar ratio of the aqueous ammonia calculated on a dry basis to the silver source calculated on a silver ion basis is 1-5:1.

[0040] Preferably, in step (1), the conditions of the first contact reaction include at least: a temperature of 30-70° C. and a time of 30-60 min.

[0041] Preferably, in step (1), the directing agent is an aqueous solution of sodium sulfide and / or an aqueous solution of sodium hydrosulfide.

[0042] According to a particularly preferred embodiment of the present invention, in step (1), the molar ratio of the amount of the silver source calculated as silver ions to the amount of the directing agent calculated as dry basis is 1:0.001-0.01. In the present invention, in the process of synthesizing ultrafine silver powder, the yield of rod-shaped silver particles can be increased by adding sodium sulfide (Na2S) and / or sodium bisulfide (NaHS). When the concentration of the added sulfide is too high, Ag2S will be produced, and the Ag2S nanoparticles catalyze the reduction of Ag ions by significantly reducing the reduction potential. On the other hand, the presence of sulfide anions can accelerate the polyol synthesis of silver nanocubes, so that the reduction rate of silver ions is significantly increased. However, the inventors have found that the molar ratio of the amount of the silver source calculated as silver ions to the amount of the directing agent calculated as dry basis is 1:0.001-0.01, combined with the other technical features of the technical solution provided by the present invention, can make the yield of ultrafine silver powder higher and the monodispersity better.

[0043] Preferably, in step (2), the capping agent is a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 2.3-3.6:1. In the present invention, the capping agent is a factor that affects the growth kinetics of liquid phase synthesis. A higher concentration of PVP leads to isotropic coverage of the seed surface and the formation of rod-shaped silver nanoparticles. However, the inventors have found that by controlling the molar ratio of polyvinyl pyrrolidone to ethylenediaminetetraacetic acid in the capping agent within the range of 2.3-3.6:1, combined with the other technical features of the technical solution provided by the present invention, it is possible to establish a balance between adsorption and desorption on the surface of the silver growth particles, thereby obtaining ultrafine silver powder with an average particle size that meets the requirements.

[0044] Preferably, in step (2), the number average molecular weight of the polyvinyl pyrrolidone is not greater than 15,000.

[0045] Preferably, in step (2), the conditions of the second contact reaction include at least: a temperature of 50-80° C. and a time of 30-60 min.

[0046] According to a particularly preferred embodiment of the present invention, in step (2), the dispersant is triethanolamine.

[0047] Preferably, in step (2), the molar ratio of the dispersant to the capping agent is 1:3-5.

[0048] Preferably, in step (2), the conditions of the third contact reaction include at least: temperature of 60-100° C., pressure of 0.3-0.6 MPa, and time of 50-100 min.

[0049] As mentioned above, the second aspect of the present invention provides rod-shaped ultrafine silver powder prepared by the method described in the first aspect.

[0050] As mentioned above, the third aspect of the present invention provides the use of the rod-shaped ultrafine silver powder described in the second aspect in the preparation of conductive silver paste.

[0051] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the experimental instruments and raw materials involved are all commercially available.

[0052] The raw materials involved in the following examples are all analytically pure chemical reagents.

[0053] Reducing agent I: a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.025:1;

[0054] Reducing agent II: a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.032:1;

[0055] Reducing agent III: a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.05:1;

[0056] Reducing agent IV: a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.1:1;

[0057] Reducing agent V: a combination of hydroquinone and ethylene glycol in a molar ratio of 0.025:1;

[0058] Directing agent I: sodium sulfide aqueous solution;

[0059] Directing agent II: sodium hydrosulfide aqueous solution;

[0060] Capping agent I: a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 3:1;

[0061] Capping agent II: a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 3.6:1;

[0062] Capping agent III: a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 4:1;

[0063] Polyvinyl pyrrolidone: brand PVP360, purchased from Sigma-aldrich;

[0064] Dispersant: triethanolamine, analytical grade reagent.

[0065] Example 1

[0066] This embodiment provides a method for preparing rod-shaped ultrafine silver powder, the method comprising:

[0067] (1) at 40° C., 100 mL of a 0.15 mol / L silver nitrate solution, 200 mL of a 0.2 mol / L reducing agent I and 70 mL of a 0.5 mol / L ammonia solution are contacted and reacted for 50 min to obtain a mixed solution I;

[0068] (2) The mixed solution I, 3 mL of a directing agent I with a concentration of 0.02 mol / L, 4 mol of a capping agent I and 1 mol of a dispersant are reacted at normal pressure for 40 min at 60° C., and then reacted in a high-pressure reactor at 80° C. and 0.5 MPa for 70 min. The final reaction product is diluted with acetone, collected by centrifugation, and finally rinsed with water, and then suspended in water with a volume 100 times that of the silver powder to obtain rod-shaped ultrafine silver powder S1.

[0069] Example 2

[0070] This embodiment provides a method for preparing rod-shaped ultrafine silver powder, the method comprising:

[0071] (1) at 60° C., 100 mL of a 0.075 mol / L silver nitrate solution, 200 mL of a 0.12 mol / L reducing agent II and 70 mL of a 0.5 mol / L ammonia solution were contacted and reacted for 40 min to obtain a mixed solution I;

[0072] (2) At 80° C., the mixed solution I, 3 mL of a directing agent I with a concentration of 0.02 mol / L, 4 mol of a capping agent I and 1 mol of a dispersant are reacted at normal pressure for 30 min, and then reacted in a high-pressure reactor at 100° C. and 0.5 MPa for 50 min. The final reaction product is diluted with acetone, collected by centrifugation, and finally rinsed with water, and then suspended in water with a volume 100 times that of the silver powder to obtain rod-shaped ultrafine silver powder S2.

[0073] Example 3

[0074] This embodiment provides a method for preparing rod-shaped ultrafine silver powder, the method comprising:

[0075] (1) at 70° C., 100 mL of a 0.15 mol / L silver nitrate solution, 200 mL of a 0.2 mol / L reducing agent III and 70 mL of a 0.5 mol / L ammonia solution were contacted and reacted for 30 min to obtain a mixed solution I;

[0076] (2) At 50° C., the mixed solution I, 3 mL of a directing agent II with a concentration of 0.02 mol / L, 4 mol of a capping agent II and 1 mol of a dispersant are reacted at normal pressure for 60 min, and then reacted in a high-pressure reactor at 60° C. and 0.4 MPa for 80 min. The reaction product is diluted with acetone, collected by centrifugation, and finally rinsed with water, and then suspended in water with a volume 100 times that of the silver powder to obtain rod-shaped ultrafine silver powder S3.

[0077] Example 4

[0078] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (1), reducing agent I was replaced by reducing agent IV in an equal volume.

[0079] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder S4.

[0080] Example 5

[0081] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (2), the capping agent I was replaced by an equimolar amount of the capping agent III.

[0082] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder S5.

[0083] Example 6

[0084] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (1), the concentration of the silver nitrate solution used was 0.3 mol / L.

[0085] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder S6.

[0086] Example 7

[0087] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (1), the concentration of the reducing agent I used was 0.3 mol / L.

[0088] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder S7.

[0089] Comparative Example 1

[0090] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (1), the reducing agent I was replaced by an equimolar amount of hydrazine hydrate.

[0091] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder DS1.

[0092] Comparative Example 2

[0093] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (2), an equimolar amount of polyvinyl pyrrolidone was used to replace the capping agent I.

[0094] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder DS2.

[0095] Comparative Example 3

[0096] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (1), the concentration of the silver nitrate solution used was 0.6 mol / L.

[0097] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder DS3.

[0098] Comparative Example 4

[0099] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (1), the concentration of the reducing agent I used was 0.5 mol / L.

[0100] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder DS4.

[0101] Comparative Example 5

[0102] Rod-shaped ultrafine silver powder was prepared according to the method of Example 1, except that in step (1), reducing agent I was replaced by reducing agent V in an equal volume.

[0103] The remaining steps are the same as those in Example 1 to obtain rod-shaped ultrafine silver powder DS5.

[0104] Test Example 1

[0105] The rod-shaped ultrafine silver powders prepared in the examples and comparative examples were subjected to performance tests, and the specific test results are shown in Table 1.

[0106] The test method for the average particle size and particle size distribution is as follows: according to the method described in the standard GB / T19077.1-2008 / ISO13320-1, the particle size and particle size distribution of the ultrafine silver powder are tested using a Mastersizer 3000 laser particle size analyzer;

[0107] The impurity content test method is: according to the method described in standard GB / T11067-2006, the impurity content in the ultrafine silver powder is tested using a WFX-120B atomic absorption spectrophotometer.

[0108] Table 1

[0109]

[0110]

[0111] It can be seen from the results in the above table that the average particle size of the ultrafine silver powder prepared by the method provided by the present invention is significantly reduced, the particle size distribution is narrow, and it can be close to monodisperse ultrafine silver powder, and the impurity content in the ultrafine silver powder can also be significantly reduced; in particular, the average particle size of the ultrafine silver powder is reduced to below 0.3 μm.

[0112] Test Example 2

[0113] The rod-shaped ultrafine silver powders prepared in the examples and comparative examples were made into silver wire electrodes, and the conductivity of the obtained silver wire electrodes was tested. The specific test results are shown in Table 2.

[0114] Among them, the preparation method of the silver wire electrode is: the rod-shaped ultrafine silver powder, oxide binder (Bi2O3) and organic carrier (composed of ethyl cellulose and ethyl 2-(2-n-butoxyethoxy)acetate in a mass ratio of 1:1) prepared in the embodiment and the comparative example are mixed in a mass ratio of 72:8:20, and the ultrafine silver powder is evenly dispersed by ultrasonic dispersion and three-roll mill mixing to prepare a conductive silver paste. The conductive silver paste is printed on an alumina substrate by a screen printer. The silver paste printed electrode is linear, with a line width of about 60μm, a line spacing of about 80μm, and a silver paste film wet film thickness of about 40μm. The silver paste film is dried under an infrared lamp at 150°C and sintered in a BTU furnace at 250°C for 30 minutes with a standard 60-minute cycle. The sintered film thickness is about 15μm to prepare a silver wire electrode;

[0115] The test method of electrical conductivity is: according to the method described in the national standard JJG376-2007, the electrical conductivity of the silver wire electrode is tested by the Loresta-GXMCP-T700 conductivity tester using the DC four-probe method.

[0116] Table 2

[0117]

[0118]

[0119] It can be seen from the results in the above table that the conductive silver paste formed by the ultrafine silver powder prepared by the method provided by the present invention has high electrical conductivity.

[0120] The rod-shaped ultrafine silver powder prepared in Example 1 of the present invention was placed under a scanning electron microscope (model Sirion200, purchased from FEI Company) equipped with an energy dispersive x-ray analyzer to observe the microstructure of the ultrafine silver powder, and was placed on an x-ray diffractometer with CuKα radiation (model X′ProMPD, purchased from Philip Company) for analysis. The analysis results are shown in FIG. Figure 1 and Figure 2 .

[0121] Figure 1 is a scanning electron microscope characterization image of the rod-shaped ultrafine silver powder prepared in Example 1 of the present invention, Figure 2 This is an X-ray diffraction characterization diagram of the rod-shaped ultrafine silver powder prepared in Example 1 of the present invention.

[0122] from Figure 1 It can be seen that the ultrafine silver powder prepared by the method of the present invention mainly exists in the form of particles, the shape of the silver particles is an obvious rod-like structure, the silver powder has no obvious agglomeration phenomenon, most of the silver particles exist in a monodisperse form, and the particle size distribution of the silver particles is relatively uniform.

[0123] from Figure 2 It can be seen that there are four diffraction peaks at 2θ of 35° to 80°. Compared with the standard spectrum of metallic silver, they correspond to the diffraction peaks of four crystal planes, namely (111), (200), (220), and (311), of face-centered cubic phase metallic silver, and there are no other impurity peaks; that is, it is shown that the method provided by the present invention can prepare single-phase silver particles with a cubic structure.

[0124] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing rod-shaped ultrafine silver powder, characterized in that: The method includes: (1) in the presence of aqueous ammonia, subjecting a silver source and a reducing agent to a first contact reaction to obtain a mixed solution I; (2) in the presence of a dispersant, subjecting the mixed solution I, the directing agent and the capping agent to a second contact reaction and a third contact reaction in sequence; Wherein, in step (1), the reducing agent is a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.01-0.2:1; the concentration of the silver source in terms of silver ions is 0.01-0.5 mol / L, and the concentration of the reducing agent is 0.02-0.4 mol / L; In step (2), the capping agent is a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 0.5-5:

1.

2. The method according to claim 1, characterized in that In step (1), the reducing agent is a combination of hydrazine hydrate and ethylene glycol in a molar ratio of 0.02-0.05:

1.

3. The method according to claim 1, characterized in that In step (1), the concentration of the silver source in terms of silver ions is 0.05-0.2 mol / L, and the concentration of the reducing agent is 0.05-0.2 mol / L.

4. The method according to any one of claims 1 to 3, characterized in that: In step (1), the conditions of the first contact reaction include at least: a temperature of 30-70° C. and a time of 30-60 min.

5. The method according to any one of claims 1 to 3, characterized in that: In step (2), the directing agent is a sodium sulfide aqueous solution and / or a sodium hydrosulfide aqueous solution; and / or In step (2), the molar ratio of the silver source calculated as silver ions to the directing agent calculated as dry basis is 1:0.001-0.

01.

6. The method according to any one of claims 1 to 3, characterized in that: In step (2), the capping agent is a combination of polyvinyl pyrrolidone and ethylenediaminetetraacetic acid in a molar ratio of 2.3-3.6:

1.

7. The method according to any one of claims 1 to 3, characterized in that: In step (2), the number average molecular weight of the polyvinyl pyrrolidone is not greater than 15,000.

8. The method according to any one of claims 1 to 3, characterized in that: In step (2), the conditions of the second contact reaction include at least: a temperature of 50-80°C and a time of 30-60 min; and / or In step (2), the conditions of the third contact reaction include at least: temperature of 60-100° C., pressure of 0.3-0.6 MPa, and time of 50-100 min.

9. Rod-shaped ultrafine silver powder prepared by the method according to any one of claims 1 to 8.

10. Use of the rod-shaped ultrafine silver powder according to claim 9 in preparing conductive silver paste.