Sodium ion battery and preparation of sodium vanadium fluorophosphate electrode material
By using complex precipitation method in the preparation of sodium ion battery positive electrode materials, the problems of low vanadium source conversion and poor product crystallinity are solved, and efficient and low-cost preparation of vanadium phosphate is achieved, which is suitable for sodium ion battery positive electrodes. Materials improve electrochemical properties.
Patent Information
- Application Number
- CN202310435660.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-21
AI Technical Summary
In the preparation method of the existing sodium ion battery positive electrode material, sodium vanadium fluorophosphate, the vanadium source conversion rate is low, the product crystallinity is poor, and the morphology is irregular, resulting in waste of vanadium resources and high production costs, and it is difficult to ensure uniformity and good product. Crystal shape.
Complex precipitation method is used to form a mixed solution in low-temperature aqueous solution, and the vanadium source, sodium source, phosphate root source and fluorine source, and the precipitation reaction temperature and time are controlled and the dynamics of the reaction system are optimized. Equilibration to produce high crystallinity sodium vanadium fluorophosphate.
It has achieved efficient utilization of vanadium resources, reduced energy consumption and production costs, significantly improved the crystallinity and yield of sodium vanadium fluorophosphate, and is suitable for sodium ion battery positive electrode materials, improving electrochemical performance.
Smart Images

Figure HDA0004192121340000011 
Figure HDA0004192121340000012 
Figure HDA0004192121340000021
Abstract
Description
Technical Field
[0001] The invention relates to a battery electrode material, in particular to a method for preparing sodium vanadium fluorophosphate used as a positive electrode material for a sodium ion battery. Background Art
[0002] The current trend of global energy transformation is to shift from fossil fuel energy to a low-carbon energy system, and eventually enter the era of renewable energy. Promoting the development of renewable energy can not only provide a safe guarantee for sustainable development, but also has important practical significance in alleviating climate warming, reducing extreme weather, and reducing environmental pollution. However, due to natural conditions, the power output of major renewable energy sources such as photovoltaics, wind power, and tides often exhibits randomness, volatility, and instability. Once the power is directly output, it will bring a huge impact on the power grid and be accompanied by a large power loss. Therefore, in order to increase the safety and sustainability of energy supply, it is necessary to develop an efficient and stable large-scale energy storage system. Among many energy storage systems, electrochemical energy storage has high working efficiency and low development and maintenance costs.
[0003] At present, lithium battery still accounts for the largest proportion of electrochemical energy storage. However, due to the research bottlenecks encountered in the development of lithium-ion batteries themselves and the limited lithium resources in the world, people have turned their attention to the sodium-ion battery system.
[0004] There are three main types of positive electrode materials for sodium ion batteries: transition metal oxides, Prussian blue (white) compounds, and polyanion compounds. In response to the application needs of the energy storage market (no resource restrictions, long life, high safety, etc.), the polyanion positive electrode material system has advantages in raw material resource utilization, processing, safety, and cycle life. Since the polyanion positive electrode material system does not have the problem of residual alkali on the surface of the oxide positive electrode material system, it is easier to control the storage and production environment during material storage and battery processing, and the production cost is greatly reduced. In these aspects, the polyanion positive electrode material system has obvious advantages over other positive electrode material systems.
[0005] CN107154493A discloses a method for preparing sodium vanadium fluorophosphate synthesized in a low-temperature, normal-pressure aqueous solution. Although sodium vanadium fluorophosphate is successfully prepared, the conversion rate of the vanadium source is generally very low, resulting in a low yield of the product sodium vanadium fluorophosphate, which causes a waste of the vanadium source and is not conducive to reducing costs; in addition, the crystallinity of the sodium vanadium fluorophosphate is low, impurity phases are generated, and the product morphology is irregular, and the uniformity and good crystal form of the product sodium vanadium fluorophosphate cannot be guaranteed.
[0006] CN114933293A realizes the synthesis of sodium vanadium fluorophosphate by atmospheric pressure water precipitation reaction by introducing alkali solution into the reaction mixture. Although the precipitation reaction time is shortened and the preparation efficiency and product yield are improved, the prepared sodium vanadium fluorophosphate has poor crystallinity, uneven particle size, serious agglomeration and irregular morphology. This is because its nucleation rate is fast, which is not conducive to crystal growth, and the reaction is easy to generate a large amount of amorphous flocs. Summary of the invention
[0007] The object of the present invention is to provide a method for preparing sodium vanadium fluorophosphate which is particularly suitable for use as a positive electrode material for sodium ion batteries.
[0008] According to a first aspect of the present invention, there is provided a method for preparing sodium vanadium fluorophosphate used as an electrode material, comprising:
[0009] Providing a trivalent or tetravalent vanadium source, wherein the vanadium source is provided by at least one of vanadium dioxide, vanadium oxychloride, vanadium oxysulfate (or its hydrate), vanadium oxyoxalate (or its hydrate), vanadium trioxide, vanadium trichloride, vanadium tribromide and vanadium triiodide;
[0010] providing a sodium source, wherein the sodium source is provided by at least one of sodium fluoride, sodium dihydrogen phosphate (or its hydrate), disodium hydrogen phosphate (or its hydrate), sodium phosphate (or its hydrate), sodium oxalate, sodium carbonate, sodium bicarbonate, sodium chloride, sodium bromide, sodium iodide, sodium citrate and sodium hydroxide;
[0011] providing a phosphate source, wherein the phosphate source is provided by at least one of phosphoric acid, sodium dihydrogen phosphate (or its hydrate), ammonium dihydrogen phosphate, disodium hydrogen phosphate (or its hydrate), diammonium hydrogen phosphate, sodium phosphate (or its hydrate), and ammonium phosphate (or its hydrate);
[0012] providing a fluorine source, wherein the fluorine source is provided from at least one of sodium fluoride, ammonium fluoride and hydrofluoric acid;
[0013] A vanadium source, a sodium source, a phosphate source and a fluorine source are formed into a mixed solution;
[0014] Providing a complex precipitant, wherein the complex precipitant is provided by at least one of urea, ammonia water, sodium oxalate, sodium citrate, sodium ascorbate, sodium tartrate, sodium lactate, lysine, sodium glutamate and vanadyl oxalate (or its hydrate);
[0015] The complex precipitant is continuously added into the mixed solution at a uniform speed to carry out precipitation reaction to obtain sodium vanadium fluorophosphate precipitate, wherein the continuous addition time is 10min-4h, and the reaction temperature is 60℃-120℃.
[0016] According to the preparation method of the present invention, the complexing precipitant is preferably added for 1-3 hours, more preferably about 2 hours. The precipitation reaction temperature is preferably 80° C.-100° C., more preferably about 90° C. In addition, after the complexing precipitant is added, the reaction can be continued for 10-50 minutes.
[0017] According to the preparation method of the present invention, the vanadium source is preferably at least one tetravalent vanadium source selected from vanadium dioxide, vanadium dichloride, vanadium sulfate (or its hydrate), and vanadium oxalate (or its hydrate), and more preferably vanadium sulfate (or its hydrate).
[0018] According to the preparation method of the present invention, the sodium source is preferably provided by at least one of sodium fluoride, sodium dihydrogen phosphate (or its hydrate), disodium hydrogen phosphate (or its hydrate) and sodium phosphate (or its hydrate), more preferably sodium dihydrogen phosphate or its hydrate or sodium fluoride.
[0019] According to the preparation method of the present invention, the phosphate source is preferably provided by at least one of sodium dihydrogen phosphate (or its hydrate), ammonium dihydrogen phosphate, disodium hydrogen phosphate (or its hydrate), and diammonium hydrogen phosphate, and more preferably sodium dihydrogen phosphate or its hydrate.
[0020] According to the preparation method of the present invention, the complex precipitant is preferably provided by at least one of urea, sodium oxalate, sodium citrate and vanadyl oxalate (or its hydrate), and more preferably urea.
[0021] According to a preferred specific embodiment of the preparation method of the present invention, the vanadium source is provided by vanadyl sulfate (or its hydrate), the phosphate source and part of the sodium source are provided by sodium dihydrogen phosphate or its hydrate, the fluorine source and the remaining sodium source are provided by sodium fluoride, and the complex precipitant is provided by urea.
[0022] According to the preparation method of the present invention, the molar ratio of Na:V:P:F elements in the mixed solution is preferably (3-15):2:(2-15):(1-15), and the molar ratio of the complex precipitant to the vanadium source is preferably (0.5-5):1.
[0023] According to the preparation method of the present invention, the trivalent or tetravalent vanadium source can be obtained by reducing the pentavalent vanadium source. The reducing agent can be provided by at least one of citric acid, oxalic acid, ascorbic acid, tartaric acid, lactic acid, sodium citrate, sodium oxalate, sodium ascorbate, sodium tartrate, sodium lactate, thiourea, sodium sulfite and sodium thiosulfate. The molar ratio of the pentavalent vanadium source to the reducing agent can be 1: (0.5-5); the reaction temperature after the two are mixed can be 60°C-100°C, such as 80°C; the reaction time can be 0.5-1h.
[0024] According to the preparation method of the present invention, stirring is maintained during the entire precipitation reaction process, and the stirring speed can be 100-1000r / min until the reaction is completed to obtain a light green or green precipitate. After stopping stirring, the product settles immediately and does not require aging time, and can be post-processed. The post-processing method can be: solid-liquid separation, washing and drying of the reaction mixture. The solvent used for washing can be at least one of deionized water and ethanol, and the number of washings can be 6-8 times. The drying method can be vacuum drying or drying in the air, preferably vacuum drying, the drying temperature is 50-120°C, preferably 60°C; the drying time can be 2-24h, preferably 6-12h.
[0025] According to the method of the present invention, sodium vanadium fluorophosphate can be quickly prepared in a low-temperature aqueous solution, without the need for subsequent aging treatment and high-temperature sintering process, which greatly reduces the energy consumption of the product, significantly enhances the preparation time, and thus saves economic costs. In addition, the vanadium source conversion rate is high and the product yield is high, achieving efficient utilization of the vanadium source. In addition, the prepared sodium vanadium fluorophosphate has a good crystal form and high crystallinity, and the assembled battery exhibits excellent electrochemical properties when used as the positive electrode of a sodium ion battery. In addition, the method according to the present invention does not require high temperature, high pressure, or a closed environment, and the device is simple and the process is simple, which is particularly suitable for industrial large-scale production.
[0026] According to a second aspect of the present invention, there is also provided a positive electrode material, comprising sodium vanadium fluorophosphate prepared according to the above method, wherein the chemical composition of the sodium vanadium fluorophosphate is Na3(VO 1-x PO4)2F 1+2x , where 0≤x≤1.
[0027] According to another aspect of the present invention, a sodium ion battery is provided, comprising a positive electrode made of the above-mentioned positive electrode material, wherein the chemical formula of the sodium vanadium fluorophosphate is Na3V2O2(PO4)2F.
[0028] CN107154493A and CN114933293A use solid alkali or alkali solution to adjust the pH of the reaction system: when no alkali is added, the product yield is greatly reduced, which is due to the slow reaction kinetics of the reaction system, resulting in a low vanadium source conversion rate; when a strong alkali is added, the product yield is improved and the preparation process time is shortened, but the crystallinity of the product is seriously reduced, which is due to the addition of a strong alkali solution. The system equilibrium quickly moves to the right, the reaction kinetics are greatly accelerated, the product nucleation rate is too fast, and the growth process is inhibited, resulting in poor crystallinity. The principle of the present invention may be explained as using a complex precipitation method to achieve the controlled release of free vanadium ions and phosphates, and coordinating and controlling the vanadium concentration and phosphate concentration and pH in the reaction system so that the system reaches a dynamic equilibrium to optimize the nucleation rate, so that the crystal has enough time to grow, thereby obtaining sodium vanadium fluorophosphate with high crystallinity; while ensuring a high conversion rate of the product, the aging is significantly enhanced.
[0029] In summary, compared with the prior art, the present invention has at least the following significant advantages:
[0030] The present invention can quickly prepare sodium vanadium fluorophosphate in a relatively low-temperature aqueous solution without the need for subsequent aging treatment and high-temperature sintering, thereby greatly reducing product energy consumption, shortening preparation time, and saving production costs;
[0031] The present invention controls the concentration of free vanadium ions and phosphate radicals in the reaction mixed solution by means of complex precipitation, and the prepared sodium vanadium fluorophosphate has good crystal form, high crystallinity and high yield, and is particularly suitable for use as a positive electrode material for sodium ion batteries, and the assembled battery exhibits excellent electrochemical performance;
[0032] The present invention realizes the dynamic balance of the whole reaction system by controlling the complex precipitation rate, thereby optimizing and regulating the nucleation and growth of sodium vanadium fluorophosphate crystals to obtain sodium vanadium fluorophosphate with required size and morphology.
[0033] The preparation method of the present invention does not require high temperature, high pressure, or a closed environment, has a simple device, and a simple process, and is particularly suitable for industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1-3 They are respectively the XRD pattern, SEM pattern and charge-discharge curve of Na3V2O2(PO4)2F prepared according to Example 1 of the present invention.
[0035] Figure 4 It is the XRD pattern of the product prepared according to Comparative Example 1. DETAILED DESCRIPTION
[0036] The present invention is further described below in conjunction with the examples and comparative examples of preparing sodium vanadium fluorophosphate and the accompanying drawings.
[0037] Example 1
[0038] Dissolve 2.282 g of vanadyl sulfate in 200 mL of deionized water and stir to obtain a vanadium source solution;
[0039] Add 6.552 g of sodium dihydrogen phosphate dihydrate and 1 g of sodium fluoride to the above vanadium source solution, stir evenly, and heat to 90°C;
[0040] Dissolve 2.52g urea in 200mL deionized water, stir to dissolve evenly, and then add it to the mixed solution at a uniform speed. The addition time is 2h. After the addition is completed, continue heating for half an hour to obtain a light green precipitate, and the upper liquid is almost colorless, clear and transparent;
[0041] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 2.667 g of product with a yield of 92.5%.
[0042] The obtained light green powder was subjected to XRD test, and the test results were as follows: Figure 1 The XRD results show that the product is Na3V2O2(PO4)2F, which has good crystallinity and high purity. The product was tested by scanning electron microscopy (SEM), and the test results are as follows Figure 2 The SEM results show that the product has the appearance of a "cuju" ball with a diameter of about 0.5-1um.
[0043] The obtained product Na3V2O2(PO4)2F was made into the positive electrode, and metallic sodium was used as the negative electrode to assemble a button cell. The charge and discharge curve was tested at a current density of 0.1C. The test results are as follows: Figure 3 The test results show that the material has two discharge platforms near 4.0V and 3.60V voltages, and the discharge specific capacity at 0.1C current density is about 129.9mAh / g, which is almost equal to the theoretical specific capacity of the material.
[0044] Example 2
[0045] Dissolve 2.17 g of vanadium oxalate in 200 mL of deionized water and stir to obtain a vanadium source solution;
[0046] Add 6.552 g of sodium dihydrogen phosphate dihydrate and 1 g of sodium fluoride to the above vanadium source solution, stir evenly, raise the temperature to 90°C, and heat at a constant temperature for 3 hours to obtain a light green precipitate, and the upper liquid is almost colorless, clear and transparent;
[0047] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 2.604 g of product with a yield of 90.3%.
[0048] Example 3
[0049] Dissolve 1.638 g of ammonium metavanadate and 0.938 g of sodium oxalate in 200 mL of deionized water, heat to 80 °C, and stir at constant temperature for 0.5 h;
[0050] Add 6.552 g of sodium dihydrogen phosphate dihydrate and 1 g of sodium fluoride to the above solution, stir evenly, and heat to 90°C;
[0051] Dissolve 5.628g of sodium oxalate in 200mL of deionized water, stir and dissolve evenly, then add it to the mixed solution at a uniform speed for 2 hours. After the addition is completed, continue heating for half an hour to obtain a light green precipitate, and the upper liquid is almost colorless, clear and transparent;
[0052] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 2.757 g of product with a yield of 95.6%.
[0053] Example 4
[0054] Dissolve 2.548 g of vanadium pentoxide and 1.26 g of oxalic acid in 200 mL of deionized water, heat to 80 °C, and stir at constant temperature for 0.5 h;
[0055] Add 13.104 g of sodium dihydrogen phosphate dihydrate and 2 g of sodium fluoride to the above solution, stir evenly, and heat to 90°C;
[0056] Dissolve 11.256g of sodium oxalate in 200mL of deionized water, stir and dissolve evenly, then add it to the mixed solution at a uniform speed for 2 hours. After the addition is completed, continue heating for half an hour to obtain a light green precipitate, and the upper liquid is almost colorless, clear and transparent;
[0057] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 5.468 g of product with a yield of 94.8%.
[0058] Example 5
[0059] Dissolve 2.548 g of vanadium pentoxide and 1.232 g of ascorbic acid in 200 mL of deionized water, heat to 80 °C, and stir at constant temperature for 0.5 h;
[0060] Add 13.104 g of sodium dihydrogen phosphate dihydrate and 2 g of sodium fluoride to the above solution, stir evenly, and heat to 90°C;
[0061] Dissolve 21.672g of sodium citrate in 200mL of deionized water, stir and dissolve evenly, then add it to the mixed solution at a uniform speed for 2 hours. After the addition is completed, continue heating for half an hour to obtain a light green precipitate, and the upper liquid is almost colorless, clear and transparent;
[0062] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 5.266 g of product with a yield of 91.3%.
[0063] Example 6
[0064] Dissolve 2.1 g of vanadium trioxide and 10 mL of phosphoric acid in 200 mL of deionized water;
[0065] Add 13.104 g of sodium dihydrogen phosphate dihydrate and 2 g of sodium fluoride to the above solution, stir evenly, and heat to 90°C;
[0066] Dissolve 5.04 g of urea in 200 mL of deionized water, stir to dissolve evenly, and then add it to the mixed solution at a uniform rate. The addition time is 2 hours. After the addition is completed, continue heating for half an hour to obtain a light green precipitate, and the upper liquid is almost colorless, clear and transparent;
[0067] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 5.27 g of product with a yield of 90.1%.
[0068] Comparative Example 1
[0069] Dissolve 2.282 g of vanadyl sulfate in 200 mL of deionized water and stir to obtain a vanadium source solution;
[0070] Add 6.552 g of sodium dihydrogen phosphate dihydrate and 1 g of sodium fluoride to the above vanadium source solution, stir evenly, and heat to 90°C;
[0071] Dissolve 1.484g of sodium carbonate in 200mL of deionized water, stir and dissolve evenly, then add it to the mixed solution at a uniform speed for 2 hours. After the addition is completed, continue heating for half an hour, stop stirring, and there is no obvious sedimentation phenomenon; place it at room temperature and let it stand for 12 hours, a little precipitation appears at the bottom, and the upper solution is dark brown;
[0072] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 0.472 g of product with a yield of 16.4%. The product was light gray in color.
[0073] The obtained product was subjected to XRD test, and the test results were as follows: Figure 4 The XRD results show that the product has very poor crystallinity and is amorphous, which is obviously inconsistent with the sodium vanadium fluorophosphate phase.
[0074] Comparative Example 2
[0075] Dissolve 2.282 g of vanadyl sulfate in 200 mL of deionized water and stir to obtain a vanadium source solution;
[0076] Add 6.552g of sodium dihydrogen phosphate dihydrate and 1g of sodium fluoride to the above vanadium source solution, stir evenly, heat to 90°C, continue heating for 3 hours and then stop stirring, there is no obvious sedimentation phenomenon, the upper liquid is dark blue; place it at room temperature and age it for 12 hours, a little precipitation appears at the bottom, and the upper solution is dark brown;
[0077] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60° C. for 6 h to obtain 0.540 g of product with a yield of 18.7%.
[0078] Comparative Example 3
[0079] Dissolve 2.282 g of vanadyl sulfate in 200 mL of deionized water and stir to obtain a vanadium source solution;
[0080] Add 6.552 g of sodium dihydrogen phosphate dihydrate and 1 g of sodium fluoride to the above vanadium source solution, stir evenly, and heat to 90°C;
[0081] Dissolve 2.52g urea in 200mL deionized water, stir and dissolve evenly, then pour directly into the above mixed solution, continue heating for 3 hours and then stop stirring, no obvious sedimentation phenomenon; leave it at room temperature for 12 hours, a little precipitation appears at the bottom, and the upper solution is dark brown;
[0082] The precipitate was washed three times with deionized water and ethanol respectively, and then dried under vacuum at 60°C for 6 h to obtain 0.571 g of product with a yield of 19.8%.
[0083] The comparative examples show that when the urea complexing precipitant is not used in the reaction system or is not added in a controlled and continuous manner, the crystallinity of the product formed is extremely poor and the vanadium conversion rate is extremely low. This is probably related to the inability to achieve a controlled release of the free vanadium ion and phosphate concentration in the mixed solution.
Claims
1. A method for preparing sodium vanadium fluorophosphate used as an electrode material, comprising: providing vanadyl sulfate as a vanadium source; providing sodium dihydrogen phosphate as a phosphate source and part of the sodium source, and providing sodium fluoride as a fluoride source and the remaining sodium source; A vanadium source, a sodium source, a phosphate source and a fluorine source are formed into a mixed solution, wherein the molar ratio of the elements Na:V:P:F in the mixed solution is (3-15):2:(2-15):(1-15), and the molar ratio of the complexing precipitant to the vanadium source is (0.5-5):1; providing urea as a complexing precipitant; The complex precipitant is continuously added to the mixed solution at a uniform speed to carry out precipitation reaction to obtain sodium vanadium fluorophosphate precipitate, wherein the continuous addition time is 1h-3h, and the reaction temperature is 80°C-100°C.
Citation Information
Patent Citations
Preparation of sodium vanadium fluorophosphate and application of sodium vanadium fluorophosphate in sodium ion battery
CN114933293A
Sodium vanadium fluorophosphate, preparation method and uses thereof
CN107154493A