A method for oxygen-free dehydrogenation of methanol

Through the high-entropy metal oxide catalyst, the oxygen-free dehydrogenation reaction in a fixed bed reactor, the existing catalyst stability and selectivity problems are solved, and the efficient preparation of anhydrous formaldehyde and hydrogen co-production are achieved, with the highest formaldehyde yield reaching 81.5%.

CN116217360BActive Publication Date: 2024-11-05DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111479282.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-06
Publication Date
2024-11-05
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

The existing oxide catalysts have short stability, good selectivity but low conversion rate in methanol dehydrogenation reaction, and their selectivity decreases at high temperatures, making it difficult to effectively prepare anhydrous formaldehyde and co-produced hydrogen.

Method used

Using a high entropy metal oxide catalyst, the catalyst consists of MgCoNiCuZnOx, LiMgCoNiZnOx, etc., by performing an oxygen-free dehydrogenation reaction with methanol at a certain temperature and pressure in a fixed bed reactor, and diluting it with inert gas to generate formaldehyde and produce hydrogen in parallel. High entropy oxides of different structures are prepared and cooled by high temperature smelting.

Benefits of technology

The high efficiency of methanol-free dehydrogenation is achieved in preparing anhydrous formaldehyde, the catalyst has good stability and high formaldehyde yield, up to 81.5%, and can maintain high-efficiency reaction at relatively low pressures and temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003394783350000101
    Figure BDA0003394783350000101
Patent Text Reader

Abstract

The present invention relates to a method for oxygen-free dehydrogenation of methanol, and more particularly to a method for synthesizing anhydrous formaldehyde from methanol under oxygen-free inert conditions. The process is carried out in a fixed bed reactor, and methanol undergoes a dehydrogenation reaction on a high entropy oxide catalyst to generate formaldehyde. Since neither the raw material nor the product contains water, the obtained formaldehyde is anhydrous formaldehyde, and hydrogen is co-produced in the process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a catalytic method for oxygen-free dehydrogenation of methanol, and in particular to a catalytic oxygen-free dehydrogenation method for methanol on a high-entropy metal oxide. Background Art

[0002] Formaldehyde is an important bulk organic chemical raw material, and its production process is relatively mature. At present, the production of formaldehyde is mainly prepared by methanol oxidation method, which can be roughly divided into: iron molybdenum method and silver method according to the catalyst used, but the formaldehyde produced by these two methods is 38-55% formaldehyde aqueous solution. Too high water content of formaldehyde will affect the preparation of downstream engineering plastics, dyes, hexamethyleneimine (urotropine) and polyoxymethylene dimethyl ether and other products. Anhydrous formaldehyde has higher economic value and wider market demand.

[0003] Methanol dehydrogenation can generate formaldehyde and methyl formate, and can also be cracked into CO and H2. From a thermodynamic point of view, methanol dehydrogenation is an endothermic reaction. Only when the reaction temperature is higher than 400°C can a meaningful methanol conversion rate be obtained. When the temperature is higher than 600°C, the methanol conversion rate can reach more than 95%. The direct dehydrogenation of methanol to formaldehyde is a volume increase reaction, so increasing the reaction pressure is not conducive to the reaction. The higher the reaction pressure, the smaller the equilibrium constant and the lower the equilibrium conversion rate. Therefore, the reaction should be carried out at normal pressure or lower pressure as much as possible. In addition, from a kinetic point of view, formaldehyde dehydrogenation is several orders of magnitude higher than methanol dehydrogenation. Therefore, methanol dehydrogenation selectively generates formaldehyde. The reaction depends on external energy supply and the use of highly active and highly selective catalysts. At the same time, the contact time should be shortened as much as possible during the reaction to reduce the occurrence of side reactions and quickly condense the product.

[0004] With the rapid development of the methanol industry and the increasing market demand for anhydrous formaldehyde, there is an urgent need to accelerate the development of methanol dehydrogenation to formaldehyde process. The key to its industrialization lies in the design and synthesis of catalysts.

[0005] The oxide catalysts that are currently being studied more include CuO / SiO2 and ZnO / SiO2, but the main problem with these catalysts is that the stability time is too short. Researchers mainly extend the life of the catalyst by adding additives or changing the preparation method of the catalyst. For example, by adding Cr additives, the aggregation of Cu crystallites is dispersed and inhibited, and the oxidation state of Cu is stabilized. The selectivity of metal oxide catalysts is good, but the conversion rate is not high and the life is not long, and the selectivity will decrease when the conversion rate is increased by increasing the temperature. In particular, due to the generation of reducing gases such as CO and H2 in the methanol dehydrogenation reaction, the active components of the oxide catalyst will gradually be reduced to metals and evaporate and lose, thereby losing the activity of the catalyst. Therefore, it is very necessary to enhance the reduction resistance of the oxide catalyst.

[0006] High entropy metal oxides have high resistance to reduction, and using high entropy metal oxides as catalysts to catalyze the anaerobic dehydrogenation of methanol to produce anhydrous formaldehyde has advantages. Summary of the invention

[0007] The problem to be solved by the present invention is to provide a method for anaerobic dehydrogenation of methanol, starting from cheap, readily available and stable methanol, through a high entropy oxide catalyst, through catalytic dehydrogenation under anaerobic conditions to prepare anhydrous formaldehyde and co-produce hydrogen.

[0008] The technical solution is:

[0009] In a fixed bed reactor, methanol is gasified and diluted with an inert gas or undiluted, and then reacts on a certain amount of high entropy oxide catalyst under certain temperature and pressure conditions to produce formaldehyde. No water is produced during the reaction, and hydrogen is co-produced.

[0010] The inert atmosphere includes: N2, Ar, He or a mixture thereof;

[0011] The inert gas accounts for 20-90% of the total volume of the total gas;

[0012] The mass space velocity of methanol on the catalyst is: 0.5-5h -1 ;

[0013] Reaction temperature: 500-750°C;

[0014] Reaction pressure: 0.5-5atm.

[0015] The inert atmosphere includes: N2;

[0016] The inert gas accounts for 40-80% of the total volume of the total gas;

[0017] The mass space velocity of methanol on the catalyst is: 0.5-2h -1 ;

[0018] Reaction temperature: 600-750℃;

[0019] Reaction pressure: 0.5-3atm.

[0020] The inert gas accounts for 50-60% of the total volume of the total gas;

[0021] The mass space velocity of methanol on the catalyst is: 1-3h -1 ;

[0022] Reaction temperature: 650-750℃;

[0023] Reaction pressure: 0.5-1atm.

[0024] The high entropy oxide catalyst is a fluorite-type, spinel-type, layered O3-type, or rock salt-type high entropy oxide.

[0025] The high entropy oxide catalyst is MgCoNiCuZnO x Composition of high entropy oxide, LiMgCoNiZnO x Composition of high entropy oxide, LiMgCoNiCuZnO x Composition of high entropy oxide, LiTiCrMnCoNbO x Composition of high entropy oxide, MgTiFeCuZnO x Composition of high entropy oxide, NaMgCoNiCuO x Composition of high entropy oxide, TiMnFeSnSbO x A high entropy oxide of composition, where x is any value that satisfies the stoichiometric ratio.

[0026] The preparation method of the high entropy oxide catalyst is to mix the metal precursor salts constituting the high entropy oxide in a certain proportion, stir and ball-mill them evenly, and then place them in a high-temperature melting furnace under a certain temperature and a certain atmosphere for a certain period of time, immediately take them out, and then place them in a cold environment to cool. The obtained samples are high entropy oxides of different compositions.

[0027] The metal precursor salts constituting the high entropy oxide include solid metal carbonates, nitrates, oxalates, ammonium salts, sulfates, and acetates thereof;

[0028] The molar ratio of any two elements corresponding to the elements constituting the high entropy oxide is: 0.9 to 1.1;

[0029] The temperature of the high temperature smelting furnace is 600-1500°C;

[0030] The gas used in the smelting process is one of air, oxygen, or an inert gas containing 5-99.9% oxygen, or a mixture thereof;

[0031] The smelting process lasts for 1-60 minutes;

[0032] The cold environment includes: room temperature air, dry ice environment, liquid nitrogen environment or other available cold environments that do not react with high temperature oxides.

[0033] Beneficial technical effects

[0034] 1. The present invention uses an innovative high entropy oxide catalyst component design to achieve anaerobic dehydrogenation of methanol to produce anhydrous formaldehyde and co-produce hydrogen with cheap, readily available and simple raw materials;

[0035] 2. The catalyst has good stability, the reaction process is simple, controllable and easy to operate, and the yield of formaldehyde can reach up to 81.5%. DETAILED DESCRIPTION

[0036] In order to further explain the present invention in detail, several specific implementation cases are given below, but the present invention is not limited to these embodiments.

[0037] Example 1

[0038] According to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1, magnesium nitrate, cobalt nitrate, nickel nitrate, copper nitrate and zinc nitrate were weighed and mixed. After being fully stirred and ball-milled to mix evenly, the mixture was placed in a 600℃ smelting furnace and air-treated for 60 minutes. It was immediately taken out and cooled under room temperature air conditions. The sample obtained after cooling was recorded as MgCoNiCuZnO x X-ray diffraction (XRD) characterization shows that its structure is a rock salt phase composite oxide.

[0039] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 20% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 650°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 4 hours of reaction are shown in Table 1.

[0040] Example 2 (using the catalyst sample in Example 1)

[0041] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 40% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 650°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 4 hours of reaction are shown in Table 1.

[0042] Example 3 (using the catalyst sample in Example 1)

[0043] The obtained sample was pressed into tablets with a mesh size of 20-60 and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 650°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 4 hours of reaction are shown in Table 1.

[0044] Example 4 (using the catalyst sample in Example 1)

[0045] The obtained sample was pressed into tablets with a mesh size of 20-60 and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 80% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 650°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 4 hours of reaction are shown in Table 1.

[0046] Example 5 (using the catalyst sample in Example 1)

[0047] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 90% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 650°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 4 hours of reaction are shown in Table 1.

[0048] Example 6

[0049] Lithium carbonate, magnesium carbonate, cobalt carbonate, nickel nitrate and zinc nitrate were weighed according to the metal ion molar ratio of 0.9 / 1 / 1 / 1 / 1.1, and the mixture was fully stirred and ball-milled to mix evenly. The mixture was placed in a smelting furnace at 800°C, and oxygen was introduced for 30 minutes. The mixture was immediately taken out and cooled in dry ice. The sample obtained after cooling was recorded as LiMgCoNiZnO x X-ray diffraction (XRD) characterization shows that its structure is a rock salt phase composite oxide.

[0050] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas Ar. The volume of inert gas accounted for 50% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 700°C and 1 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 6 hours of reaction are shown in Table 1.

[0051] Example 7 (using the catalyst sample in Example 6)

[0052] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas Ar. The volume of inert gas accounted for 50% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 1 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 6 hours of reaction are shown in Table 1.

[0053] Example 8 (using the catalyst sample in Example 6)

[0054] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas Ar. The volume of inert gas accounted for 50% of the total gas volume. The mass space velocity of methanol on the catalyst was 2h -1 The reaction was carried out at 700°C and 1 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 6 hours of reaction are shown in Table 1.

[0055] Example 9 (using the catalyst sample in Example 6)

[0056] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas Ar. The volume of inert gas accounted for 50% of the total gas volume. The mass space velocity of methanol on the catalyst was 3h -1 The reaction was carried out at 700°C and 1 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 6 hours of reaction are shown in Table 1.

[0057] Example 10 (using the catalyst sample in Example 6)

[0058] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas Ar. The volume of inert gas accounted for 50% of the total gas volume. The mass space velocity of methanol on the catalyst was 5h -1 The reaction was carried out at 700°C and 1 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 6 hours of reaction are shown in Table 1.

[0059] Embodiment 11

[0060] Lithium carbonate, magnesium carbonate, cobalt carbonate, nickel nitrate, copper nitrate and zinc nitrate were weighed according to the metal ion molar ratio of 1 / 0.9 / 0.9 / 1 / 1 / 1, and the mixture was fully stirred and ball-milled to mix evenly. The mixture was placed in a 1000℃ melting furnace, and 5% O2 and N2 mixed gas was introduced for 20 minutes. It was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as LiMgCoNiCuZnO x X-ray diffraction (XRD) characterization shows that its structure is a rock salt phase composite oxide.

[0061] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas He. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 500°C and 0.7 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0062] Example 12 (using the catalyst sample in Example 11)

[0063] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas He. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 0.7 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0064] Example 13 (using the catalyst sample in Example 11)

[0065] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas He. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 650°C and 0.7 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0066] Example 14 (using the catalyst sample in Example 11)

[0067] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas He. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.7 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0068] Example 15 (using the catalyst sample in Example 11)

[0069] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas He. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 750°C and 0.7 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0070] Example 16

[0071] Lithium carbonate, titanium sulfate, chromium nitrate, manganese carbonate, cobalt carbonate and ammonium niobium oxalate were weighed according to the metal ion molar ratio of 1 / 0.9 / 0.9 / 0.9 / 1 / 1, and the mixture was fully stirred and ball-milled to mix evenly. The mixture was placed in a 1200℃ melting furnace, and 10% O2 and Ar mixed gas was introduced for 10 minutes. It was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as LiTiCrMnCoNbO x X-ray diffraction (XRD) characterization shows that its structure is a fluorite-type composite oxide.

[0072] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0073] Example 17 (using the catalyst sample in Example 16)

[0074] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 1 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0075] Example 18 (using the catalyst sample in Example 16)

[0076] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 2 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0077] Example 19 (using the catalyst sample in Example 16)

[0078] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 3 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 3 h of reaction are shown in Table 1.

[0079] Embodiment 20

[0080] According to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1, magnesium carbonate, titanium sulfate, iron nitrate, copper nitrate and zinc nitrate were weighed, and after being fully stirred and ball-milled to mix evenly, the mixture was placed in a 1500℃ smelting furnace, and 99.9% O2 and He mixed gas was introduced for 1 minute, and then it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as MgTiFeCuZnO x X-ray diffraction (XRD) characterization shows that its structure is a spinel-type composite oxide.

[0081] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0082] Embodiment 21

[0083] Sodium carbonate, magnesium carbonate, cobalt nitrate, nickel nitrate and copper nitrate were weighed according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1, and the mixture was fully stirred and ball-milled to mix evenly. The mixture was placed in a 1000℃ melting furnace, and after air treatment for 10 minutes, it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as NaMgCoNiCuO x X-ray diffraction (XRD) characterization shows that its structure is a layered O3-type phase composite oxide.

[0084] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0085] Embodiment 22

[0086] Titanium sulfate, manganese nitrate, iron nitrate, tin nitrate and antimony acetate were weighed according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1, and the mixture was fully stirred and ball-milled to mix evenly. The mixture was placed in a 1000℃ melting furnace, and after air treatment for 10 minutes, it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as TiMnFeSnSbO x X-ray diffraction (XRD) characterization shows that its structure is a rock salt phase composite oxide.

[0087] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 48 hours of reaction are shown in Table 1.

[0088] Comparative Example 1

[0089] Copper nitrate was placed in a 1000℃ melting furnace, air was introduced for 10 minutes, and then it was taken out immediately and cooled in liquid nitrogen. The sample obtained after cooling was recorded as CuO x .

[0090] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0091] Comparative Example 2

[0092] Nickel nitrate and copper nitrate were weighed at a metal ion molar ratio of 1 / 1, and after being fully stirred and ball-milled to mix evenly, the mixture was placed in a 1000°C melting furnace, and after being treated with air for 10 minutes, it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as NiCuO x XRD characterization showed that it was a mixture of Ni and Cu oxides.

[0093] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0094] Comparative Example 3

[0095] Magnesium carbonate, nickel nitrate, and copper nitrate were weighed at a metal ion molar ratio of 1 / 1 / 1, and the mixture was thoroughly stirred and ball-milled to mix evenly. The mixture was placed in a 1000°C melting furnace, and after air treatment for 10 minutes, it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as MgNiCuO x XRD characterization showed that it was a mixture of oxides of Mg, Ni and Cu.

[0096] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0097] Comparative Example 4

[0098] TiCl3 solution, ammonium metavanadate, ZrO(NO3)3, ammonium niobium oxalate and ammonium molybdate were weighed according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1, and the mixture was fully stirred and ball-milled to mix evenly. The mixture was placed in a 1000℃ melting furnace, and after air treatment for 10 minutes, it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as TiVZrNbMoO x , XRD characterization shows that it is a mixture of Ti, V, Zr, Nb, and Mo oxides.

[0099] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0100] Comparative Example 5

[0101] Mg(NO3)2, TiCl3 solution, Fe(NO3)3, Co(NO3)2, Ni(NO3)2, and ZrO(NO3)3 were weighed according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1 / 1. After being fully stirred and ball-milled to mix evenly, the mixture was placed in a 1000℃ melting furnace, and after being treated with air for 10 minutes, it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as MgTiFeCoNiZrO x , XRD characterization shows that it is a mixture of oxides of Mg, Ti, Fe, Co, Ni, and Zr.

[0102] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0103] Comparative Example 6

[0104] TiCl3 solution, ammonium metavanadate, Cr(NO3)3, Fe(NO3)3, Co(NO3)2, and ZrO(NO3)2 were weighed according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1 / 1. After being fully stirred and ball-milled to mix evenly, the mixture was placed in a 1000℃ melting furnace, and after being treated with air for 10 minutes, it was immediately taken out and placed in liquid nitrogen for cooling. The sample obtained after cooling was recorded as TiVCrFeCoZrO x , XRD characterization shows that it is a mixture of oxides of Ti, V, Cr, Fe, Co, and Zr.

[0105] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was gasified and diluted with inert gas N2. The volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 700°C and 0.5 atm and monitored online by gas chromatography. The yield and selectivity of the formaldehyde product after 24 hours of reaction are shown in Table 1.

[0106] Table 1 Reaction evaluation results

[0107]

[0108]

[0109] From Examples 1-5, it can be seen that the higher the volume of inert gas, the higher the conversion rate and the higher the selectivity. Considering the reaction efficiency, it is more appropriate to select an inert gas volume ratio of 50-60%. From Examples 6-10, it can be seen that the higher the methanol mass space velocity, the lower the conversion rate and the lower the selectivity. Considering the efficiency of the reaction, it is better to select 1 to 3. From Examples 11-15, it can be seen that the higher the reaction temperature, the higher the conversion rate, but the lower the selectivity. The suitable temperature range is 650-750°C. From Examples 16-18, it can be seen that the higher the reaction pressure, the lower the conversion rate and the lower the selectivity. The optimal range is 0.5-1atm. From Comparative Examples 1-3 and Example 21, it can be seen that the activity of single-component, two-component and three-component metal oxide catalysts is not as good as that of high-entropy metal oxide catalysts. From Comparative Examples 4, 5, and 6, it can be seen that multi-component metal oxides of other element combinations cannot form composite oxides with specific crystal structures. They are mixtures of simple metal oxides and have poor catalytic performance.

Claims

1. A method for anaerobic dehydrogenation of methanol, characterized in that: In a fixed bed reactor, the raw material methanol is gasified, diluted with an inert gas or not, and then reacts on a high entropy oxide catalyst with a specific crystal structure of the following specific elements to generate formaldehyde. No water is produced during the reaction, and hydrogen is co-produced at the same time. The reaction temperature is: 500-750 ℃; The crystal structure of the high entropy oxide catalyst is one or more of fluorite type, spinel type, layered O3- type, and rock salt type; The high entropy oxide is a high entropy oxide composed of six specific elements of iron, cobalt, nickel, copper, zinc and oxygen, a high entropy oxide composed of six specific elements of lithium, magnesium, cobalt, nickel, zinc and oxygen, a high entropy oxide composed of seven specific elements of lithium, magnesium, cobalt, nickel, copper, zinc and oxygen, a high entropy oxide composed of seven specific elements of lithium, titanium, chromium, manganese, cobalt, niobium and oxygen, a high entropy oxide composed of six specific elements of magnesium, titanium, iron, copper, zinc and oxygen, a high entropy oxide composed of six specific elements of sodium, magnesium, cobalt, nickel, copper and oxygen, a high entropy oxide composed of six specific elements of titanium, manganese, iron, tin, antimony and oxygen, and one or more of the above high entropy oxides, wherein the molar proportion of the oxygen element is the molar proportion of oxygen that satisfies the stoichiometric ratio required by all metal elements; The preparation method of the high entropy oxide catalyst is as follows: the metal precursor salts constituting the high entropy oxide are mixed in proportion, stirred and ball-milled evenly, and then placed in a high-temperature smelting furnace for treatment, immediately taken out, and then placed in a cold environment for cooling; the obtained samples are high entropy oxides of different compositions; the high entropy oxide catalyst is MgCoNiCuZnO x Composition of high entropy oxide, LiMgCoNiZnO x Composition of high entropy oxide, LiMgCoNiCuZnO x Composition of high entropy oxide, LiTiCrMnCoNbO x Composition of high entropy oxide, MgTiFeCuZnO x Composition of high entropy oxide, NaMgCoNiCuO x Composition of high entropy oxide, TiMnFeSnSbO x A high entropy oxide composed of, wherein x is any value satisfying the stoichiometric ratio; the metal precursor salt constituting the high entropy oxide is selected from one or more of its solid metal carbonates, nitrates, oxalates, ammonium salts, sulfates, and acetates; The molar ratio between any two elements of the metal elements constituting the high entropy oxide is 0.9-1.1; the temperature of the high-temperature smelting furnace is 600-1500°C; the processing time is more than 1 minute; The gas used in the smelting process is one of air, oxygen, or an inert atmosphere containing 5-99.9% oxygen by volume, or a mixture thereof; the inert atmosphere is selected from one or more of N2, Ar, and He; The smelting process lasts for 1-60 min.

2. The method according to claim 1, characterized in that: The inert atmosphere is selected from: one or more of N2, Ar, and He; The inert gas accounts for 20-90% of the total volume of the total gas, and the total gas is methanol and the inert gas; The mass space velocity of methanol on the catalyst is: 0.5-5 h -1 ; Reaction pressure: 0.5-5 atm.

3. The method according to claim 1, characterized in that: The inert atmosphere is selected from: N2; The inert gas accounts for 40-80% of the total volume of the total gas; The mass space velocity of methanol on the catalyst is: 0.5-2 h -1 ; Reaction temperature: 600-750 °C; Reaction pressure: 0.5-3 atm.

4. The method according to claim 1, 2 or 3, characterized in that: The inert gas accounts for 50-60% of the total volume of the total gas; The mass space velocity of methanol on the catalyst is: 1-3 h -1 ; Reaction temperature: 650-750 °C; Reaction pressure: 0.5-1 atm.

5. The method according to claim 1, characterized in that: The molar ratio between any two elements corresponding to the metal elements constituting the high entropy oxide is: 0.95-1.05; The temperature of the high temperature smelting furnace is 800-1300°C; The cold environment is selected from: one or more of room temperature air, dry ice environment, and liquid nitrogen environment.