An electrically responsive acrylic acid ion exchange resin and its preparation method and application

By introducing carbon nanotubes into the electrically responsive acrylic ion exchange resin and combining electrochemical methods, the secondary pollution caused by high concentration of acid during adsorbent regeneration is solved, and efficient copper ion recovery under low concentration of acid conditions is achieved. It enhances the mechanical strength and adsorption capacity of the resin, and provides a green and efficient heavy metal ion recovery method.

CN116218019BActive Publication Date: 2024-11-05SHENZHEN RES INST OF NANJING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310235083.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-11-05
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

The prior art requires a large number of chemical reagents in the regeneration process of heavy metal ion adsorbents, which leads to secondary pollution problems and is difficult to effectively recover metal ions, affecting resource utilization.

Method used

The electrically responsive acrylic ion exchange resin introduced by carbon nanotubes is used to achieve the regeneration and recovery of metal ions under low concentration acid conditions through electrochemical methods, and the mechanical strength and adsorption capacity of the resin are enhanced by using the carbon nanotube network.

Benefits of technology

It realizes efficient recovery of copper ions under low concentration acid conditions, reduces the use of chemical reagents, improves the mechanical strength and adsorption amount of resin, reduces secondary pollution, and provides a green and efficient heavy metal ion recovery method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116218019B_ABST
    Figure CN116218019B_ABST
Patent Text Reader

Abstract

The invention discloses an electrically responsive acrylic acid ion exchange resin and a preparation method and application thereof. Carbon nanotubes are introduced in situ into the polymerization reaction of acrylic acid monomers through in-situ suspension polymerization, and then further hydrolyzed to obtain an electrically responsive acrylic acid ion exchange resin. The invention uses polyacrylic acid as a skeleton and introduces carbon nanotubes in situ into the polymerization reaction process to obtain an electrically responsive acrylic acid resin. The electrically responsive acrylic acid ion exchange resin has higher mechanical strength and can adsorb Cu 2+ in water. 2+ , and can use its inductive effect to assist with a small amount of acid to recover copper ions in a green way. It overcomes the secondary pollution problem caused by a large amount of chemical reagents in the regeneration process of traditional metal ion adsorbents, and provides new materials and methods for the resource recovery of heavy metal wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an electrically responsive acrylic acid series ion exchange resin and a preparation method and application thereof, and belongs to the field of sewage treatment and resource control. Background Art

[0002] After metal ions are enriched in the human body, they will affect human health. For example, the discharge of heavy metal copper ions in wastewater is extremely harmful to water bodies and soil. In addition, excessive copper in the human body will burden the liver and gallbladder. Therefore, with the increasing severity of heavy metal pollution, it is particularly important to find economical, green and environmentally friendly methods for heavy metal treatment. In addition, it is worth noting that copper-containing wastewater is mainly wastewater generated by industries such as metallurgy and electronics. 2+ The discharge not only pollutes the environment, but also causes waste of resources. At present, the main treatment methods for heavy metal ions are adsorption, flocculation and sedimentation, membrane separation technology, biological methods, etc. Adsorption separation has been used for heavy metal treatment in wastewater for decades due to its simple operation and good treatment effect. Moreover, with the development of many new and efficient adsorbents, the advantages of low cost, high capacity, and fast kinetics have been achieved. However, in the process of adsorbent regeneration, it is often necessary to add acid (2~3M) with hundreds to thousands of times the pollutant content, resulting in acid with more complex components, making it difficult to recover metal ions, and further supporting desorption liquid technology for deep treatment is required. Therefore, the study of green and efficient adsorbent regeneration technology is of great significance for recovering heavy metal ions in wastewater and improving economic benefits.

[0003] The acrylic anion exchange resin skeleton contains a large number of carboxyl groups, which can adsorb, chelate or exchange heavy metal ions. At the same time, acrylic ion exchange resins are highly recyclable and environmentally friendly, playing an important role in heavy metal polluted wastewater. Existing studies have shown that acrylic ion exchange resins are effective for Cu 2+ It has a high adsorption capacity, but its regeneration still requires a high amount of acid, which is not environmentally friendly. Electrochemical technology can change the interaction between the adsorbent and the adsorbate by regulating the surface charge state of the material, essentially weakening and dismantling the interaction between the adsorbent and the adsorbate, and achieving the regeneration of metal ions without consuming or reducing chemical reagents. However, acrylic resin is an insulating material and cannot play its advantages in the field of electrochemistry. Therefore, it is urgent to solve the secondary pollution problem caused by high concentration of acid in the process of regenerating and recovering metal ions by resin adsorption. Summary of the invention

[0004] Purpose of the invention: The first purpose of the present invention is to provide an electrically responsive acrylic ion exchange resin. The second purpose of the present invention is to provide a method for preparing the electrically responsive acrylic ion exchange resin. The third purpose of the present invention is to provide an application of the electrically responsive acrylic ion exchange resin in electrochemical recovery of metallic copper ions in water.

[0005] Technical solution: A method for preparing an electrically responsive acrylic ion exchange resin of the present invention comprises the following steps:

[0006] (1) Placing carbon nanotubes (CNTs) in a benign resin porogen, dispersing them by ultrasonication at a constant temperature, and obtaining a carbon nanotube suspension:

[0007] (2) mixing and stirring the reaction monomer, the cross-linking agent, the initiator and the carbon nanotube suspension to dissolve to obtain an oil phase solution;

[0008] (3) placing a dispersant and sodium chloride in deionized water, heating and stirring to dissolve, to obtain an aqueous solution;

[0009] (4) adding the oil phase solution to the water phase solution under heating and stirring, adjusting the stirring, slowly raising the temperature to react, and continuing to raise the temperature to mature, to obtain resin beads;

[0010] (5) The resin beads are washed with hot water and ethanol for several times, extracted with petroleum ether, and vacuum dried to obtain dry resin beads;

[0011] (6) The dried resin beads are placed in a sodium hydroxide solution, heated for reaction, washed with water until neutral, and dried to obtain an electrically responsive acrylic ion exchange resin.

[0012] Furthermore, in step (1), the carbon nanotubes have a length of 30 to 50 μm and an inner diameter of 10 to 20 nm.

[0013] Furthermore, in step (1), the benign porogen is toluene.

[0014] Furthermore, in step (1), the solid-liquid ratio of the carbon nanotubes to the benign porogen is 0.5 to 10 mg / mL.

[0015] Furthermore, in step (1), the heat preservation and ultrasonic dispersion time is 10 to 30 minutes.

[0016] Furthermore, in step (2), the monomer, cross-linking agent and initiator are methyl methacrylate, divinylbenzene and azobisisobutyronitrile, respectively.

[0017] Furthermore, in step (2), the mass ratio of the monomer, the cross-linking agent, the initiator and the carbon nanotube is 1:0.15:0.01:0.001-0.02.

[0018] Furthermore, in step (3), the dispersant is polyvinyl alcohol.

[0019] Furthermore, in step (3), the mass ratio of the dispersant to sodium chloride is 1:1 to 5.

[0020] Furthermore, in step (3), the heating and stirring dissolution is to heat the mixture to 35-40° C. and reflux and stir for 0.5-1 h.

[0021] Furthermore, in step (4), the mass ratio of the oil phase solution to the water phase solution is 6 to 2:1.

[0022] Furthermore, in step (4), the slow temperature increase reaction is to slowly increase the temperature to 70-75° C. and keep the temperature for 2-4 hours.

[0023] Furthermore, in step (41), the continued heating and maturation is to heat the mixture to 85-80° C. and mature the mixture for 3-5 hours.

[0024] Furthermore, in step (4), the stirring is adjusted to adjust the stirring until the diameter of the oil droplets is 0.6 to 1 mm.

[0025] Furthermore, in step (6), the concentration of the sodium hydroxide solution is 3 mol / L.

[0026] Furthermore, in step (6), the solid-to-liquid ratio of the dried resin beads to the sodium hydroxide solution is 0.1 to 0.2 g / mL.

[0027] Furthermore, in step (6), the temperature of the heating reaction is 60 to 70° C., and the time of the heating reaction is 6 to 8 hours.

[0028] The electrically responsive acrylic acid-based ion exchange resin obtained by the preparation method of the present invention is used in electrochemical recovery of metallic copper ions in water.

[0029] Furthermore, after the metal ions are adsorbed, an external potential of 2 to 5 V is applied, assisted by the addition of a hydrochloric acid solution, so that the electrically responsive acrylic ion exchange resin can be recovered and the metal ions can be concentrated and recovered.

[0030] Furthermore, the metal ion concentration multiple is 1.5 to 11.9.

[0031] The present invention uses polyacrylic acid as a skeleton and introduces carbon nanotubes in situ into its polymerization reaction process to prepare an electrically responsive acrylic resin. The electrically responsive acrylic ion exchange resin has higher mechanical strength and can adsorb Cu 2+ in water. 2+, and can use its inductive effect to assist with a small amount of acid to recover copper ions in a green way. It overcomes the secondary pollution problem caused by a large amount of chemical reagents in the regeneration process of traditional metal ion adsorbents, and provides new materials and methods for the resource recovery of heavy metal wastewater.

[0032] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0033] (1) The electrically responsive acrylic ion exchange resin prepared by the present invention is black in appearance and is constructed of a carbon nanotube network inside. It is used as an adsorbent to remove Cu in water. 2+ The adsorption capacity can reach 190 mg / g, and due to the introduction of carbon nanotubes, the electrically responsive acrylic ion exchange resin prepared by the present invention has better mechanical strength. The mechanical strength of the prepared electrically responsive acrylic resin increases by 1.8 to 9.8 times.

[0034] (2) The electrically responsive acrylic ion exchange resin prepared by the present invention has good practical application value in wastewater resource utilization. Different from the regeneration of traditional resins, the electrically responsive acrylic ion exchange resin of the present invention has good electrical response and can achieve the purpose of resin regeneration and concentrated recovery of copper ions under the condition of adding low-concentration acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a photograph of the appearance of the electrically responsive acrylic ion exchange resin obtained in Example 1;

[0036] Figure 2 This is a scanning electron microscope image of the electrically responsive acrylic ion exchange resin obtained in Example 1;

[0037] Figure 3 The graph showing the change in mechanical strength of electrically responsive acrylic ion exchange resins with different carbon nanotube contents;

[0038] Figure 4 The electroresponsive acrylic ion exchange resin obtained in Example 2 was used to electro-regenerate and recover Cu under the conditions of 5V+0.1M HCl and 0.1M HCl. 2+ 's effect diagram. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0040] Example 1

[0041] (1) Weigh 10 mg of carbon nanotubes (CNTs) and place them in 20 mL of toluene solution, place them in a high-energy ultrasonic crusher for 15 min, and then cool them to obtain a toluene suspension of carbon nanotubes;

[0042] (2) Weigh 8.5 g of methyl acrylate, 1.5 g of divinylbenzene, 0.1 g of azobisisobutyronitrile and the above carbon nanotube toluene suspension, stir and dissolve to obtain an oil phase solution for later use;

[0043] (3) Weigh 0.6 g of polyvinyl alcohol and dissolve it in 60 mL of deionized water. After it is completely dissolved, add 3.0 g of NaCl, stir to dissolve, and then slowly transfer to a 250 mL three-necked flask. After slowly heating to 40° C. in a water bath, reflux and stir for 0.5 h to obtain an aqueous phase solution.

[0044] (4) Slowly add the oil phase solution obtained in step (2) into a three-necked flask, adjust the stirring speed to an oil droplet size of 0.6 mm, stabilize for 20 minutes, slowly heat to 70° C., and keep warm for 3 hours; then slowly heat to 85° C. and mature the resin for 3.5 hours; after the reaction is completed, collect the obtained resin beads;

[0045] (5) The resin beads were washed with hot water and ethanol to remove the unreacted reagents on the surface, and then placed in a gauze bag for ethanol extraction for 14 hours, and then dried to obtain dry resin beads for use;

[0046] (6) The resin beads dried in step (5) are placed in 50 mL of 3 mol / L sodium hydroxide solution at 60° C., slowly stirred mechanically for 6 hours, and then washed with deionized water until neutral, thereby obtaining an electrically responsive acrylic ion exchange resin (the mass percentage of carbon nanotubes in the electrically responsive acrylic ion exchange resin is 0.1%). Figure 1 The apparent photograph of the electrically responsive acrylic ion exchange resin obtained in Example 1 is Figure 1 It can be seen that the prepared acrylic acid ion exchange resin appears to be black spherical particles.

[0047] The electroresponsive acrylic ion exchange resin obtained in this example was analyzed by scanning electron microscope. Figure 2 shown. Figure 2 The scanning electron microscope image of the electrically responsive acrylic ion exchange resin obtained in Example 1 is Figure 2 It can be seen that the carbon nanotubes are evenly distributed inside the resin, overlapping and entangled with each other, and many polyacrylic acid blocks appear on the surface.

[0048] According to the above method, the electrically responsive acrylic ion exchange resins containing carbon nanotubes of 0% (no carbon nanotubes), 0.5%, 1.0%, 1.5% and 2% by mass were prepared. The mechanical strength of the electrically responsive acrylic ion exchange resins (containing carbon nanotubes 0%-2%) obtained above was tested using a particle strength tester. The results are as follows: Figure 3 shown. Figure 3 The figure shows the mechanical strength change of acrylic ion exchange resin with different contents of carbon nanotubes in electrical response. Figure 3It can be seen that due to the introduction of carbon nanotubes (CNTs), the mechanical strength of the electrically responsive acrylic ion exchange resin increases. When only 0.1% of CNTs are added, the mechanical strength of the electrically responsive acrylic ion exchange resin increases by 1.8 times (relative to 0% without adding CNTs). When 2% of CNTs are added, the mechanical strength of the electrically responsive acrylic ion exchange resin can increase by 9.8 times. The electrically responsive acrylic ion exchange resin (containing 0.1% carbon nanotubes) prepared in this example is used as an adsorbent, and the treatment concentration is 50 mg / L Cu 2+ The metal ion simulated wastewater has a pH of 5.6.

[0049] The specific operations are as follows:

[0050] Weigh 50 mg of electrically responsive acrylic acid ion exchange resin adsorbent and add it to 100 mL of 100 mg / L Cu 2+ The solution was placed in a 200 mL conical flask and adsorbed at room temperature for 18 h. 2+ The removal rate is 85.6%, and the adsorption capacity is 171.2 mg / g;

[0051] Another 125 mg of electrically responsive acrylic acid ion exchange resin was placed in an electrical regeneration column (resin column in CN2018103485394), and Cu with a pH of 5.6 and a concentration of 5 mg / L was introduced at a flow rate of 1 mL / min. 2+ After adsorption penetration, the saturated electroresponsive acrylic ion exchange resin was filled into the electroregeneration column, and 100 mL of deionized water containing 0.1 M hydrochloric acid was added. The anode potential was 2.0 V and the flow rate was 0.5 mL / min. Cu 2+ The highest concentration ratio is 1.5 times relative to the inlet concentration of 5 mg / L.

[0052] Example 2

[0053] (1) Weigh 200 mg of carbon nanotubes, place them in 20 mL of toluene solution and perform high-energy ultrasound for 30 min, then cool to room temperature to obtain a toluene suspension of carbon nanotubes for later use;

[0054] Step (2) and step (3) are the same as steps (2) and step (3) in Example 1;

[0055] (4) Slowly add the oil phase solution obtained in step (2) into a three-necked flask, adjust the stirring speed to an oil droplet size of 0.6 mm, stabilize for 20 minutes, slowly heat to 75° C., and keep warm for 3 hours; then slowly heat to 85° C. and mature the resin for 3.5 hours; after the reaction is completed, collect the obtained resin beads;

[0056] (5) The resin beads are washed with hot water and ethanol to remove the unreacted reagents on the surface, and then placed in a gauze bag for ethanol extraction for 14 hours, and then dried to obtain dry resin beads for use;

[0057] Step (6) is the same as step (6) in Example 1.

[0058] The electrically responsive acrylic acid ion exchange resin prepared in this example was used as an adsorbent to treat Cu with a concentration of 200 mg / L. 2+ The metal ion simulated wastewater has a pH of 5.6.

[0059] The specific operations are as follows:

[0060] Weigh 50 mg of electrically responsive acrylic acid ion exchange resin adsorbent and add it to 100 mL of 100 mg / L Cu 2+ The solution was placed in a 200 mL conical flask and adsorbed at room temperature for 18 h. 2+ The removal rate is 96.3%, and the adsorption capacity is 182.6 mg / g;

[0061] Another 125 mg of electrically responsive acrylic acid ion exchange resin was placed in an electrical regeneration column (the resin column in CN2018103485394). The specific process was the same as in Example 1. After the adsorption was completed, the saturated electrically responsive acrylic acid ion exchange resin was taken out and filled into the self-assembled electrical regeneration column. 100 mL of a deionized water solution containing 0.1 M hydrochloric acid was added, and a potential of 3.0 V was applied to the anode at a flow rate of 0.5 mL / min to obtain Cu 2+ The highest concentration ratio reached 5.2 times relative to the inlet concentration of 5 mg / L.

[0062] Parallel test: The electrically responsive acrylic acid ion exchange resin prepared in this example was used as an adsorbent to treat a Cu concentration of 200 mg / L. 2+ The metal ion simulated wastewater has a pH of 5.6.

[0063] The specific operations are as follows:

[0064] Weigh 50 mg of electrically responsive acrylic acid ion exchange resin adsorbent and add it to 100 mL of 100 mg / L Cu 2+ The solution was placed in a 200 mL conical flask and adsorbed at room temperature for 18 h. 2+ The removal rate is 91.8%, and the adsorption capacity is 189.6 mg / g;

[0065] Another 125 mg of electrically responsive acrylic acid ion exchange resin adsorbent was weighed and placed in an electrical regeneration column (the resin column in CN2018103485394). The specific process was the same as in Example 1. 200 mL of 5 mg / L Cu 2+The solution was used as the adsorption solution for continuous column adsorption experiments with a column flow rate of 1.0 mL / min. After the adsorption was completed, the saturated electrically responsive acrylic acid ion exchange resin was filled into the self-assembled electrical regeneration column, a potential of 5.0 V was applied to the anode, the flow rate was 0.5 mL / min, 100 mL of 0.1 M HCl aqueous solution was introduced, and desorption and recovery were performed only under 0.1 M HCl open circuit. The results are shown in FIG. Figure 4 shown. Figure 4 Electro-regeneration of Cu by electro-responsive acrylic ion exchange resin at 5V+0.1M HCl and 0.1M HCl 2+ , where (a) is the electro-responsive acrylic ion exchange resin under 5V+0.1M HCl conditions for the electro-regeneration recovery of Cu 2+ (b) is the effect diagram of the electro-responsive acrylic ion exchange resin under 0.1M HCl conditions for the electro-regeneration recovery of Cu 2+ The effect diagram. Figure 4 It can be seen that the electroresponsive acrylic ion exchange resin can be used to electroregenerate and recover Cu under the conditions of 5V+0.1M HCl (a). 2+ , get Cu 2+ The maximum concentration of Cu was 11.9 times; while the Cu 2+ The maximum concentration multiple is only 4.6 times.

Claims

1. A method for preparing an electrically responsive acrylic ion exchange resin, characterized in that: The following steps are involved: (1) placing carbon nanotubes in a benign porogen, dispersing the carbon nanotubes by ultrasonication at a constant temperature to obtain a carbon nanotube suspension, wherein the benign porogen is toluene; (2) mixing and stirring the reaction monomer methyl acrylate, the crosslinking agent, the initiator and the carbon nanotube suspension to dissolve and obtain an oil phase solution; the mass ratio of the methyl acrylate, the crosslinking agent, the initiator and the carbon nanotubes is 8.5:1.5:0.1:0.01 or 8.5:1.5:0.1:0.2; (3) placing the dispersant and sodium chloride in deionized water, heating and stirring to dissolve, and obtaining an aqueous phase solution; (4) Add the oil phase solution to the water phase solution under heating and stirring, adjust the stirring, slowly increase the temperature to react, and continue to increase the temperature and mature to obtain resin beads; (5) The resin beads are washed with hot water and ethanol for several times, extracted with petroleum ether, and vacuum dried to obtain dry resin beads; (6) placing the dried resin beads in a sodium hydroxide solution, heating for reaction, washing with water until neutral, and drying to obtain an electrically responsive acrylic ion exchange resin, wherein the concentration of the sodium hydroxide solution is 3 mol / L, the solid-liquid ratio of the dried resin beads to the sodium hydroxide solution is 0.1-0.2 g / mL, the temperature of the heating reaction is 60-70 °C, and the time of the heating reaction is 6-8 h.

2. The method for preparing the electrically responsive acrylic ion exchange resin according to claim 1, characterized in that: In step (1), the carbon nanotubes have a length of 30-50 μm and an inner diameter of 10-20 nm, and the solid-liquid ratio of the carbon nanotubes to the benign porogen is 0.5-10 mg / mL; and the heat preservation and ultrasonic dispersion time is 10-30 min.

3. The method for preparing the electrically responsive acrylic ion exchange resin according to claim 1, characterized in that: In step (2), the crosslinking agent and initiator are divinylbenzene and azobisisobutyronitrile, respectively.

4. The method for preparing the electrically responsive acrylic ion exchange resin according to claim 1, characterized in that: In step (3), the dispersant is polyvinyl alcohol, and the mass ratio of the dispersant to sodium chloride is 1:1-5. The heating and stirring dissolution is heating to 35°C-40°C, reflux and stirring for 0.5-1 h.

5. The method for preparing the electrically responsive acrylic ion exchange resin according to claim 1, characterized in that: In step (4), the mass ratio of the oil phase solution to the aqueous phase solution is 6-2:1, the slow temperature increase reaction is to slowly increase the temperature to 70-75°C and keep the temperature for 2-4 hours, and the continued temperature increase aging is to increase the temperature to 85-80°C and mature for 3-5 hours.

6. The method for preparing the electrically responsive acrylic ion exchange resin according to claim 1, characterized in that: In step (4), the stirring is adjusted to adjust the stirring until the diameter of the oil droplets is 0.6-1 mm.

7. Use of the electrically responsive acrylic ion exchange resin obtained by the preparation method according to any one of claims 1 to 6 in electrochemical recovery of metallic copper ions from water, characterized in that: After the metal ions are adsorbed, an external potential of 2 to 5 V is applied, and a hydrochloric acid solution is added to recover the electrically responsive acrylic ion exchange resin and concentrate the metal ions, wherein the metal ion concentration multiple is 1.5 to 11.9.