An exposed TPO waterproofing membrane and a preparation method thereof
By using components such as end silane-modified polyurethane prepolymer and dopamine-modified paratholite in TPO waterproof coils, the dispersion and weatherability of the materials are improved, and the existing TPO coils are solved in high temperature and high-gloss environments are solved. The aging problem under this method achieves the balance of flame retardant performance and mechanical properties, and is suitable for building waterproofing applications.
Patent Information
- Application Number
- CN202211098564.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-09-08
AI Technical Summary
While improving flame retardant performance, existing TPO waterproof coils are difficult to maintain or improve their mechanical properties, processing properties and thermal welding properties, and poor compatibility and dispersion of materials, resulting in aging in high temperature and high light environments, and their service life is shorten.
Using end silane-modified polyurethane prepolymer and dopamine-modified paraffinite and other components, the surface treatment of modified polymers and fillers can improve the dispersion of polypropylene and ethylene elastomers, and form a cross-penetrating network. Structure, reinforced materials weather resistance and durability.
It significantly improves the weather resistance and durability of the material, enhances the resistance to UV light and high temperature aging, ensures both flame retardant and mechanical properties, and extends service life. It is suitable for exposed waterproof applications in the construction industry.
Smart Images

Figure BDA0003838141940000021 
Figure BDA0003838141940000031 
Figure BDA0003838141940000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof building materials, and in particular to an exposed TPO waterproof coiled material and a preparation method thereof. Background Art
[0002] In recent years, the domestic waterproofing industry has developed rapidly, and the output and demand of waterproofing materials have increased year by year. At the same time, the performance requirements for waterproofing materials have become more and more stringent, and more and more material manufacturers have begun to move towards environmentally friendly new materials. Among them, thermoplastic polyolefin waterproofing membrane (TPO waterproofing membrane) has both the long-term weather resistance and durability of EPDM waterproofing membrane and the weldability of polyvinyl chloride waterproofing membrane, and does not contain any plasticizers and other harmful substances. At the same time, it also has the advantages of convenient construction, good waterproofing effect, and long service life. It has been widely recognized and used in the roof waterproofing industry. However, my country has a vast territory, the climate conditions between the north and the south are very different, and the roof environment is quite different. TPO membrane products need to face high solar loads and high temperature environments for a long time throughout their service life. According to data, under direct sunlight in summer, the temperature of the TPO membrane roof directly covered by solar panels can reach 88°C and last for 6 hours. In addition, TPO membranes are constructed by hot air welding for overlapping edges. Although the temperature of the automatic hot air welding machine is adjustable, the welding temperature set during construction often reaches about 500°C. If the welding temperature and welding speed are not set properly during the construction process, it may cause aging of the membrane, and the antioxidants, ultraviolet absorbers, and light and heat stabilizers in the TPO membrane formula system are exhausted prematurely, causing the product to fade, discolor, lose gloss on the surface, and even microcracks and hair-like cracks, which greatly reduces the expected service life of the product. This puts higher requirements on the performance of TPO waterproof membranes for exposed roofs.
[0003] TPO waterproofing membrane can obtain high breaking strength, tear strength and puncture resistance without any reinforcing polyester fiber, but because the oxygen index (OI) of TPO is only 18%, it is combustible, and dripping and smoke will occur during the combustion process, which greatly limits the application scope of TPO. In particular, as one of the important materials for roof waterproofing systems, the flame retardant properties of TPO waterproofing membrane are extremely important. Usually, when designing the formula of TPO waterproofing membrane, it is necessary to add inorganic metal hydroxides such as magnesium hydroxide, aluminum hydroxide, and aluminum hydroxide to improve its flame retardant properties and fire resistance; however, relevant studies have shown that they only show flame retardant properties for polymers at a higher filling amount (such as more than 30 parts), and it should be pointed out that this high flame retardancy is at the expense of the mechanical strength, processing properties, thermal welding and other properties of the material. Therefore, it is a technical problem that needs to be solved urgently to improve the flame retardant properties of TPO waterproofing membrane while maintaining or minimizing the loss of its mechanical properties, processing properties, and thermal welding properties. In addition, traditional TPO waterproof membranes have limited compatibility between ethylene elastomers and polypropylene, and ethylene elastomers cannot be well dispersed with polypropylene. At the same time, the surface of inorganic filler calcium carbonate is hydrophilic and oleophobic, and its compatibility and dispersion in polyolefins are poor, all of which lead to insufficient material welding strength, low-temperature bending properties, and tear strength.
[0004] Patent CN112708181A discloses a nano-modified weather-resistant TPO waterproofing membrane, which includes TPO resin, flame retardant, dispersant, modified filler and composite intercalation modification auxiliary agent, which are mixed and melt-plasticized and extruded, and then calendered, cooled and rolled up. The invention effectively reduces the surface energy of montmorillonite by modifying montmorillonite and then doping it into TPO waterproofing membrane, so that the montmorillonite interlayer changes from hydrophilic to lipophilic, and improves the dispersion effect inside the polyolefin resin. The preparation method is relatively complicated and the weather resistance needs to be further improved. Patent CN109624434A discloses a building waterproofing membrane for roofs and a preparation method thereof, involving three parts: a protective layer, a waterproof layer and an installation layer composed of TPO resin, asphalt, PVA fiber, flame retardant, dye, additives, etc. The invention can improve the tensile properties and tear strength of traditional TPO waterproofing membranes, thereby increasing the scope of use, but the formula contains a considerable amount of asphalt, the environmental friendliness of the product is greatly reduced, and the material does not show any improvement in weather resistance. Summary of the invention
[0005] In view of the problems in the prior art that TPO waterproofing membranes cannot have both high flame retardancy and high mechanical and processing properties, and have poor compatibility and dispersibility between components, the present invention provides an exposed TPO waterproofing membrane and a preparation method thereof. By introducing a terminal silyl-modified polyurethane prepolymer, not only can good dispersion between polypropylene (TPO) and ethylene elastomers (metallocene olefin polymers, high-density polyethylene) be achieved, but also surface modification of flame retardants, calcium carbonate fillers, and dopamine-modified palygorskite can be achieved to improve the dispersibility within polyolefins, thereby greatly improving the weather resistance and durability of the material.
[0006] An exposed TPO waterproofing membrane, which comprises the following raw materials in parts by weight:
[0007]
[0008]
[0009] The sum of the amounts of the above-mentioned TPO resin (polyolefin synthetic resin), metallocene olefin polymer and high-density polyethylene is 100 parts; the above-mentioned TPO resin is a copolymer of propylene, ethylene and butene, and a catalyst of a multi-active catalytic system is selected to introduce copolymerized ethylene and butene monomers into the molecular chain of propylene, and the total molar content of ethylene and butene on the molecular chain is 12%-18%, thereby effectively avoiding the chain degradation and aging failure of propylene containing tertiary carbon atoms caused by light, heat and oxygen during processing and use. The number average molecular weight of the TPO resin is 60,000 to 300,000. Preferably, when the molecular weight distribution is about 4 to 7, the system has good processing performance and welding construction performance, and has a good mixing and dispersion effect with a granulation additive.
[0010] The metallocene olefin polymer is a semi-crystalline polyethylene, which is an olefin copolymer prepared by polymerization of ethylene and α-olefin monomers by metallocene catalysts, wherein the α-olefin monomers are C6-C20 straight-chain α-olefins. The metallocene catalytic system belongs to a single-activity catalytic system, and the molecular weight distribution of the prepared polyethylene is relatively narrow, the composition and structure of the macromolecules are very uniform, the molecular structure is highly regular, and it has a high degree of crystallinity, which is conducive to improving low-temperature toughness.
[0011] The structural formula of the above-mentioned terminal silyl-modified polyurethane prepolymer is:
[0012] Wherein, R and R' are C1-C6 alkyl groups, a is an integer of 1-6, and b and c are integers of 20-1000. The apparent viscosity of the above-mentioned terminal silyl-modified polyurethane prepolymer is 35000-55000 cps (25°C); preferably, the terminal silyl-modified polyurethane prepolymer is SPUR+*1015LM or SPUR+*1050MM produced by Maitu High-Tech Materials Group.
[0013] The above-mentioned terminal silane-modified polyurethane prepolymer is liquid, and the main chain is a polyether structure. It has good compatibility with polyolefin resins and can wet the surface of powders. At the same time, silane and isocyanate groups can react with hydroxyl groups or metal ions on the surface of powders. The silane-modified polyurethane prepolymer, as a bridging structure, can not only achieve good dispersion between polypropylene and ethylene elastomers, but also can achieve surface modification of flame retardants, calcium carbonate fillers, and dopamine-modified palygorskite, thereby improving the dispersion inside polyolefins, thereby greatly improving the weather resistance and durability of the material.
[0014] If the amount of the terminal silyl-modified polyurethane prepolymer used is too small, the flame retardant, calcium carbonate filler, dopamine-modified palygorskite and polyolefin elastomer will not be well dispersed; if the amount of the terminal silyl-modified polyurethane prepolymer used is too large, the excess prepolymer may become a phase alone, which is detrimental to the performance of the entire system.
[0015] The flame retardant is any one of magnesium hydroxide and aluminum hydroxide.
[0016] The dopamine-modified palygorskite is obtained by the following method: the modified palygorskite is directly immersed in a dopamine hydrochloride aqueous solution (18-24 hours), separated, filtered and dried to obtain the dopamine-modified palygorskite with a polydopamine cross-linked composite layer attached to the surface. The dopamine-modified palygorskite can be firmly combined with the terminal silane-modified polyurethane prepolymer to form a cross-interpenetrating network structure in the form of chemical bonds, and the polydopamine on the surface gives the system excellent ultraviolet light absorption.
[0017] The antioxidant is B225 antioxidant. B225 is a mixture of antioxidant 1010 and antioxidant 168, and has outstanding processing stability and long-term protective effect on polyolefins.
[0018] The above-mentioned light stabilizer is light stabilizer 2020. Light stabilizer 2020 is a free radical capture light stabilizer, which can capture active free radicals, prevent the chain reaction from spreading, and achieve a stabilizing effect.
[0019] A method for preparing an exposed TPO waterproofing membrane comprises the following steps: (1) mixing and feeding: uniformly mixing TPO resin, metallocene olefin polymer, high-density polyethylene, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant and light stabilizer, and accurately metering and feeding the materials using a loss-in-weight metering scale; (2) plasticizing and extruding: plasticizing the raw materials uniformly mixed in step (1) by heating them in three stages of a twin-screw extruder; and injecting them into a mold through an injection molding head, and maintaining the pressure after injection; (3) cooling and molding: molding them through a molding device three-roll calender, and cooling them through conveyor line air; and winding them to obtain the exposed TPO waterproofing membrane.
[0020] The mixing conditions in the above step (1) are: mixing at 80-100° C. for 2 h using a high-speed stirrer.
[0021] In the above step (2), the melt extrusion temperature of the extruder is 165-235° C., the rotation speed is 100 rpm-500 rpm, the temperature of the mold is 90-100° C., the injection pressure is maintained at 0.4 MPa, and the injection time is 3 s.
[0022] The operating temperature of the three-roll calender in the above step (3) is 60-80°C.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] The present invention adopts the terminal silane-modified polyurethane prepolymer for the first time to achieve excellent dispersion stability of the whole system, and endows the coil with super strong cohesion and anti-ultraviolet / high temperature aging ability through dopamine-modified palygorskite, overcoming the problem of insufficient performance of existing TPO thermoplastic elastomers, and is particularly suitable for the demand of exposed waterproof coil in the construction industry. At the same time, the preparation method provided by the present invention is simple and feasible, the raw materials are easy to obtain, and it is suitable for industrial production. The prepared TPO waterproof coil has broad application development prospects. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0028]
[0029] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0030] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0031] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0032] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0033] Example 2
[0034] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0035]
[0036] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0037] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0038] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0039] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0040] Example 3
[0041] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0042]
[0043]
[0044] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0045] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0046] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0047] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0048] Example 4
[0049] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0050]
[0051]
[0052] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0053] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0054] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0055] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0056] Example 5
[0057] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0058]
[0059] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0060] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0061] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0062] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0063] Example 6
[0064] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0065]
[0066] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0067] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0068] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0069] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0070] Example 7
[0071] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0072]
[0073] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0074] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0075] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0076] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0077] Comparative Example 1 (containing no terminal silane-modified polyurethane prepolymer)
[0078] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0079]
[0080]
[0081] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0082] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer were mixed in a high-speed mixer at 80° C. for 2 h, and the materials were accurately weighed using a loss-in-weight weighing scale;
[0083] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0084] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0085] Comparative Example 2 (without dopamine-modified palygorskite)
[0086] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0087]
[0088] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0089] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed using a loss-in-weight weighing scale;
[0090] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0091] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0092] Comparative Example 3
[0093] The raw materials of a TPO waterproofing membrane provided by the present invention include the following components and the weight proportions of each component are as follows:
[0094]
[0095] The preparation process of the TPO waterproofing membrane of the present invention comprises:
[0096] (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, HDPE, terminal silane-modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine-modified palygorskite, antioxidant, and light stabilizer are mixed in a high-speed mixer at 80° C. for 2 h, and the materials are accurately weighed and added using a loss-in-weight weighing scale;
[0097] (2) Plasticizing and extruding: The raw materials are plasticized by heating in three stages of a twin-screw extruder, and the temperatures are controlled at 165° C., 205° C., and 235° C., respectively; and injected into a mold through an injection head, and pressure is maintained after injection to maintain the integrity of the finished product and prevent the molten raw material mixture from flowing back;
[0098] (3) Cooling and forming: The product is shaped by a three-roll calender with the temperatures of the first, second and third rollers set at 80°C, 70°C and 60°C respectively, and then cooled by air through a 10-meter conveyor line; the exposed TPO waterproof membrane product is rolled up.
[0099] Comparative Example 4
[0100] The TPO waterproof membrane product is prepared by adopting the formula process described in Example 1 of patent CN112708181A.
[0101] Performance Test:
[0102] The products obtained in the above embodiments and comparative examples were tested for performance according to the national standards GB 27789-2011 "Thermoplastic Polyolefin (TPO) Waterproof Membrane", GB / T2406.2-2009 "Determination of Combustion Performance of Plastics - Oxygen Index Method" and GB / T18244 "Aging Test Method for Building Waterproof Materials", wherein the thermal aging and artificial climate accelerated aging experimental conditions are higher than the national standard requirements. The results are shown in Table 1 below.
[0103] Table 1 Performance test indicators of the examples and comparative examples of the present invention
[0104]
[0105]
[0106] According to the data analysis in the above table, the mechanical properties of the TPO waterproofing membranes obtained in Examples 1 to 7 are far superior to the national standard requirements, while the mechanical properties of the comparative products can only approach or basically reach the national standard requirements. Whether it is the embodiment or the comparative example, the products can meet the standard requirements for low-temperature bending, and the membrane will not crack at minus 40°C. The oxygen index of the membrane products in the embodiment is about 30%, which belongs to the category of flame-retardant materials and has excellent flame retardant properties, while the oxygen index of the comparative products is below 27%, which belongs to the category of combustible materials. Under more stringent heat aging (130°C, 800h) and artificial climate accelerated aging (3000h) conditions, the embodiment products show unparalleled advantages in heat resistance and weather resistance, and their own mechanical properties have not been significantly reduced, and there is no color change in the appearance of the membrane, while the performance of the comparative products has been greatly reduced after aging, and the appearance of the membrane has obvious color change. In summary, the addition of end-silyl modified polyurethane prepolymer and dopamine modified palygorskite is crucial to the improvement of mechanical properties, flame retardancy, heat aging resistance, weather resistance and other properties of TPO membrane. The product prepared by the patent of this invention fully meets the requirements for waterproofing of exposed projects.
[0107] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An exposed TPO waterproof membrane, It is characterized in that The exposed TPO waterproof membrane comprises the following raw materials in parts by weight: 60-80 parts of TPO resin, 10-25 parts of metallocene olefin polymer, 5-15 parts of high-density polyethylene, 1 to 4 parts of terminal silane-modified polyurethane prepolymer, 20-40 parts of flame retardant, Calcium carbonate 25-45 parts, 2 to 8 parts of dopamine-modified palygorskite, Antioxidant 0.01~0.1 parts, Light stabilizer 0.01-0.1 part; The TPO resin is a copolymer of propylene, ethylene and butene, and the total molar content of ethylene and butene in the copolymer is 12%-18%, and the number average molecular weight of the TPO resin is 60,000-300,000; The sum of the amounts of the TPO resin, the metallocene olefin polymer and the high-density polyethylene is 100 parts; The metallocene olefin polymer is a semi-crystalline polyethylene, which is an olefin copolymer prepared by polymerization of ethylene and α-olefin monomers by a metallocene catalyst, wherein the α-olefin monomer is a C6-C20 straight-chain α-olefin; The structural formula of the terminal silane-modified polyurethane prepolymer is: Wherein, R and R' are C1-C6 alkane groups, a is an integer of 1-6, and b and c are integers of 20-1000; the apparent viscosity of the terminal silane-modified polyurethane prepolymer is 35000-55000 cps (25°C); The dopamine-modified palygorskite is obtained by the following method: the palygorskite to be modified is directly immersed in a dopamine hydrochloride aqueous solution, separated, filtered and dried to obtain the dopamine-modified palygorskite with a polydopamine cross-linked composite layer attached to the surface.
2. The exposed TPO waterproof membrane according to claim 1, Features: The flame retardant is any one of magnesium hydroxide and aluminum hydroxide.
3. The exposed TPO waterproof membrane according to claim 1, Features: The antioxidant is B225 antioxidant.
4. The exposed TPO waterproof membrane according to claim 1, Features: The light stabilizer is 2020 light stabilizer.
5. A method for preparing an exposed TPO waterproofing membrane according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) Mixing and adding materials: TPO resin, metallocene olefin polymer, high-density polyethylene, end-silyl modified polyurethane prepolymer, flame retardant, calcium carbonate, dopamine modified palygorskite, antioxidant and light stabilizer are mixed uniformly, and the materials are accurately weighed and discharged using a loss-in-weight weighing scale; (2) Plasticizing and extruding: The raw materials uniformly mixed in step (1) are plasticized after being heated in three stages by a twin-screw extruder; and injected into a mold through an injection molding head, and pressure is maintained after injection; (3) Cooling and molding: The raw materials are shaped by a three-roll calender of a shaping device, and cooled by air through a conveyor line; and rolled up to obtain an exposed TPO waterproof membrane.
6. The preparation method according to claim 5, Features: The mixing conditions in step (1) are: mixing at 80-100° C. for 2 h using a high-speed stirrer.
7. The preparation method according to claim 5, Features: In the step (2), the melt extrusion temperature of the extruder is 165-235° C., the rotation speed is 100 rpm-500 rpm, the temperature of the mold is 90-100° C., the injection pressure is maintained at 0.4 MPa, and the injection time is 3 s.
8. The preparation method according to claim 5, Features: The operating temperature of the three-roll calender in step (3) is 60-80°C.