A plant oil-based polyphenol and a method for preparing recyclable polyurethane foam using the same
Vegetable oil-based polyphenols are prepared by reacting vegetable oil with phenol compounds under the action of catalysts, and reacting with isocyanate to form a crosslinking network of phenol-carbamate bonds, which solves the problem of polyurethane foam dependence on petrochemical-based chemicals and difficulty in recycling and recycling. , realizes recyclable polyurethane foam, with excellent mechanical properties and environmental benefits.
Patent Information
- Application Number
- CN202211659917.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The production of polyurethane foam relies on petrochemical-based chemicals, resulting in resource depletion and environmental pollution, and is difficult to recycle and reuse after being discarded, resulting in high treatment costs and secondary pollution.
Vegetable oil-based polyphenols are prepared by reacting vegetable oil with phenolic compounds under the action of a catalyst, and mixed with raw materials such as isocyanate at room temperature to form recyclable polyurethane foam. The solvent-free green synthesis method is used to form phenol-carbamate Crosslinking network of bonds.
It realizes the reprocessing and recycling of vegetable oil-based polyurethane foam, with excellent mechanical and recycling performance, saves resources, protects the environment, and has simple technology and low cost.
Smart Images

Figure CN116218607B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane materials, and in particular relates to a plant oil-based polyphenol and a method for preparing a recyclable polyurethane foam using the same. Background Art
[0002] Polyurethane foam (PUF) has the advantages of low price, heat resistance, low thermal conductivity, light weight, high strength, ablation resistance, etc., and its structure and performance are easy to adjust. It is widely used in refrigeration and insulation, building energy conservation, furniture, shoes and clothing, vehicles and ships. The preparation of polyurethane foam is a thermosetting polymer foamed with polyols and isocyanates as the main raw materials under the action of various additives such as foaming agents and catalysts. At present, most of the polyols used to produce polyurethane foam are petrochemical-based chemicals. Due to the increasing depletion of oil resources, the rise in oil prices and the unreliability of supply have severely restricted the development of the polyurethane industry. Developing and finding new alternative resources, reducing the dependence of the polyurethane industry on petroleum products, and developing chemicals from renewable biomass sources have become major issues that human society must address in the new century.
[0003] At the same time, with the increasing use of polyurethane foam, the post-use treatment of the material also faces problems. Usually, polyurethane foam that has reached the end of its service life or has been discarded is difficult to recycle, resulting in high processing costs and easy secondary pollution. Therefore, the development of a recyclable polyurethane foam has an obvious supporting role in promoting energy conservation and emission reduction, green recycling and low-carbon development. Summary of the invention
[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a plant oil-based polyphenol and a preparation method thereof and an application thereof in the preparation of recyclable polyurethane foam.
[0005] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0006] A vegetable oil-based polyphenol is prepared by the following method: vegetable oil and phenolic compounds are reacted at 70-90°C for 3-5h under the action of a catalyst, and the vegetable oil-based polyphenol is obtained through purification.
[0007] Optionally, the phenolic compound is one or more of phenol, catechol, and guaiacol; the vegetable oil is one or more of tung oil, castor oil, soybean oil, palm oil, rubber seed oil, cottonseed oil, and rice bran oil.
[0008] Optionally, the mass ratio of the vegetable oil to the phenolic compound is 1:(1-2).
[0009] Optionally, the catalyst is one or more of p-toluenesulfonic acid, tetrafluoroboric acid, and phosphotungstic acid, and the amount of the catalyst accounts for 0.5-3% of the total mass of the vegetable oil and the phenolic compound.
[0010] A method for preparing recyclable polyurethane foam using the above-mentioned vegetable oil-based polyphenols comprises the following steps: mixing the vegetable oil-based polyphenols with isocyanate and an auxiliary agent for reaction at room temperature, pouring the mixture into a mold, and curing the mixture at a certain temperature to obtain a recyclable polyurethane foam; the auxiliary agent comprises a foaming agent, a stabilizer, and a catalyst.
[0011] Optionally, the raw material components include, by weight, 100 parts of vegetable oil-based polyphenol, 120 parts of isocyanate, 3 to 4 parts of stabilizer, 0.2 to 0.6 parts of amine catalyst, and 5 to 10 parts of foaming agent.
[0012] Optionally, the catalyst is N,N-dimethylcyclohexylamine; the foaming agent is one or more of HFC-141b, cyclopentane, and HFC-365mfc; and the stabilizer is a silicon-type foam stabilizer.
[0013] Optionally, the isocyanate is one or more of toluene diisocyanate, xylene diisocyanate, and polymethyl polyisocyanate.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] The present invention uses a wide range of low-cost, natural and renewable vegetable oils as raw materials, and prepares vegetable oil-based polyphenols through a solvent-free green synthesis method. The phenolic hydroxyl groups in the vegetable oil-based polyphenols react with isocyanates to form a vegetable oil-based polyurethane foam with a phenol-carbamate bond as a cross-linked network, so that it has the functions of reprocessing and recycling, and the recycling still has excellent performance; the vegetable oil-based polyurethane foam not only has excellent mechanical and recycling properties, but also uses forest resource vegetable oil as raw materials, and has the dual effects of saving resources and protecting the environment. The present invention has a simple preparation process, relatively low cost, and is green and sustainable. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 Schematic diagram of preparing tung oil-based polyphenols by Friedel-Crafts alkylation reaction of tung oil and guaiacol according to the present invention;
[0017] Figure 2 This is an infrared spectrum of the tung oil-based polyphenol obtained in Example 1 of the present invention;
[0018] Figure 3 This is a nuclear magnetic hydrogen spectrum test chart of the tung oil-based polyphenol obtained in Example 1 of the present invention;
[0019] Figure 4This is the ultraviolet spectrum of the tung oil-based polyphenol obtained in Example 1 of the present invention;
[0020] Figure 5 This is a test diagram of the apparent density and compressive strength of tung oil-based polyurethane foams of different proportions obtained in Example 1 of the present invention;
[0021] Figure 6 The invention relates to the recycling of the tung oil-based polyurethane foam obtained in Example 1 of the present invention;
[0022] Figure 7 This is a tensile strength test diagram of the tung oil-based polyurethane elastomer obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] The present invention is further described below in conjunction with specific embodiments.
[0024] Source of raw materials:
[0025] Tung oil, castor oil, soybean oil, palm oil, rubber seed oil, cottonseed oil, and rice bran oil: all purchased from the Nature Vegetable Oil Processing Factory in Nanxi District, Yibin City, industrial pure;
[0026] Isocyanate: Yantai Shunda Polyurethane Co., Ltd., industrial grade;
[0027] Polyether 4110: Shandong Bluestar Dongda Chemical Co., Ltd., industrial grade;
[0028] AK8804: Jiangsu Meside Chemical Co., Ltd., industrial pure;
[0029] The remaining raw materials are all commercially available conventional chemicals;
[0030] High-speed multifunctional pulverizer: Wuyi Haina Electric Co., Ltd., equipment model HC-200T;
[0031] Manual flat plate vulcanizing press: Jiangsu Xinhaojie Experimental Instrument Co., Ltd., specification model BD-8820-C;
[0032] Universal testing machine: Shenzhen Sansi Testing Equipment Co., Ltd., China, specification model CMT4000.
[0033] Example 1
[0034] Tung oil (100 g), guaiacol (200 g) and 3 wt% p-toluenesulfonic acid (based on the total weight of the raw materials) were added into a 100 mL three-necked flask, heated to 80 °C, and reacted for 4 h under stirring. The reaction process is shown in the schematic diagram. Figure 1After the reaction, 3 wt.% NaOH solution was added to remove the unreacted guaiacol, and the organic phase was collected and washed twice with deionized water. The organic phase was collected and the water was removed by rotary evaporation to obtain plant oil-based polyphenols (tung oil-based polyphenols).
[0035] According to the formula shown in Table 1, the synthesized vegetable oil-based polyphenol, polyether 4110 and the additives were mixed evenly according to different ratios of vegetable oil-based polyphenol and polyether 4110, and then stirred with 120 parts by mass of isocyanate for 20 seconds at a speed of 2500 r / min, poured into a mold, and aged at 60°C for 24 hours to obtain polyurethane foams, which were marked as TPU-1, TPU-2, TPU-3, TPU-4, and TPU-5. The prepared tung oil-based polyurethane foam was broken into 30-300 mesh powders using a high-speed multifunctional pulverizer, with a pulverizing power and time of 1200 W and 3 min, respectively, and then molded into a complete polyurethane elastomer using a manual flat vulcanizer, as shown in the schematic diagram. Figure 6 As shown, they are marked as TPUF-1, TPUF-2, TPUF-3, TPUF-4, and TPUF-5 respectively, and the compression conditions are 120°C, 15MPa, and 20min, thereby realizing the recyclable utilization of polyurethane foam.
[0036] Table 1 Preparation of polyurethane foam formulas with different proportions of vegetable oil-based polyphenols in Example 1
[0037] All by mass
[0038] sample Plant oil based polyphenols Polyether 4110 N,N-Dimethylcyclohexylamine AK8804 Cyclopentane Isocyanate TPU-1 100 0 0.6 3.5 6 120 TPU-2 80 20 0.6 3.5 6 120 TPU-3 60 40 0.6 3.5 6 120 TPU-4 40 60 0.6 3.5 6 120 TPU-5 20 80 0.6 3.5 6 120
[0039] Example 2
[0040] Castor oil (100 g), guaiacol (200 g) and 3 wt% of p-toluenesulfonic acid (based on the total mass of the raw materials) were added into a 100 mL three-necked flask, the temperature was raised to 80°C, and the mixture was reacted for 4 h under stirring. After the reaction, 3 wt.% of NaOH solution was added to remove the unreacted guaiacol, the organic phase was collected, and the mixture was washed with deionized water for 4 times. The organic phase was collected and the water was removed by rotary evaporation to obtain plant oil-based polyphenols (castor oil-based polyphenols).
[0041] According to the formula of TPU-3 shown in Table 1, the synthesized vegetable oil-based polyphenol, polyether 4110 and additives were mixed evenly, stirred with isocyanate for 20s, the speed was 2000r / min, poured into a mold, and aged at 60℃ for 24h to obtain castor oil-based polyurethane foam. The prepared tung oil-based polyurethane foam was broken into 30-300 mesh powder by a high-speed multifunctional pulverizer, the pulverization power and time were 1200W and 3min respectively, and then the powder was molded into a complete castor oil-based polyurethane elastomer by a manual flat vulcanizer, and the compression conditions were 120℃, 15MPa, and 20min, so as to realize the recyclable recycling of castor oil-based polyurethane foam.
[0042] Example 3
[0043] Soybean oil (100 g), guaiacol (200 g) and 3 wt% of p-toluenesulfonic acid (based on the total mass of raw materials) were added to a 100 ml three-necked flask, the temperature was raised to 80 ° C, and the reaction was carried out under stirring for 4 hours. After the reaction, 3 wt.% NaOH solution was added to remove the unreacted guaiacol, the organic phase was collected, and washed with deionized water for 3 times. The organic phase was collected and the water was removed by rotary evaporation to obtain plant oil-based polyphenols (soybean oil-based polyphenols).
[0044] According to the formula of TPU-3 shown in Table 1, the synthesized vegetable oil-based polyphenol, polyether 4110 and additives were mixed evenly, stirred with isocyanate for 20s, the speed was 2000r / min, poured into a mold, and aged at 60℃ for 24h to obtain soybean oil-based polyurethane foam. The prepared tung oil-based polyurethane foam was broken into 30-300 mesh powders by a high-speed multifunctional pulverizer, the pulverization power and time were 1200W and 3min respectively, and then the powder was molded into a complete soybean oil-based polyurethane elastomer by a manual flat vulcanizer, and the compression conditions were 120℃, 15MPa, and 20min, so as to realize the recyclable utilization of soybean oil-based polyurethane foam.
[0045] Example 4
[0046] Palm oil (100 g), guaiacol (200 g) and 3 wt% of p-toluenesulfonic acid (based on the total mass of the raw materials) were added into a 100 ml three-necked flask, the temperature was raised to 80°C, and the mixture was reacted for 4 h under stirring. After the reaction, 3 wt.% of NaOH solution was added to remove the unreacted guaiacol, the organic phase was collected, and the mixture was washed with deionized water for 4 times. The organic phase was collected and the water was removed by rotary evaporation to obtain plant oil-based polyphenols (palm oil-based polyphenols).
[0047] According to the formula of TPU-3 shown in Table 1, the synthesized vegetable oil-based polyphenol, polyether 4110 and additives were mixed evenly, stirred with isocyanate for 20s, the speed was 2000r / min, poured into a mold, and aged at 60℃ for 24h to obtain palm oil-based polyurethane foam. The prepared tung oil-based polyurethane foam was broken into 30-300 mesh powders by a high-speed multifunctional pulverizer, the pulverization power and time were 1200W and 3min respectively, and then the powder was molded into a complete palm oil-based polyurethane elastomer by a manual flat vulcanizer, and the compression conditions were 120℃, 15MPa, and 20min, so as to realize the recyclable utilization of palm oil-based polyurethane foam.
[0048] Example 5
[0049] Rubber seed oil (100 g), guaiacol (200 g) and 3 wt % of p-toluenesulfonic acid (based on the total mass of raw materials) were added to a 100 ml three-necked flask, heated to 80 ° C, and reacted for 4 hours under stirring. After the reaction, 3 wt. % NaOH solution was added to remove unreacted guaiacol, and the organic phase was collected and washed with deionized water for 34 times. The organic phase was collected and the water was removed by rotary evaporation to obtain plant oil-based polyphenols (rubber seed oil-based polyphenols).
[0050] According to the formula of TPU-3 shown in Table 1, the synthesized vegetable oil-based polyphenol, polyether 4110 and additives were mixed evenly, stirred with isocyanate for 20s, the speed was 2300r / min, poured into a mold, and aged at 60℃ for 24h to obtain rubber seed oil-based polyurethane foam. The prepared tung oil-based polyurethane foam was broken into 30-300 mesh powders by a high-speed multifunctional pulverizer, the pulverization power and time were 1200W and 3min respectively, and then the powder was molded into a complete rubber seed oil-based polyurethane elastomer by a manual flat vulcanizer, and the compression conditions were 120℃, 15MPa, and 20min, so as to realize the recyclable utilization of rubber seed oil-based polyurethane foam.
[0051] Example 6
[0052] Cottonseed oil (100 g), guaiacol (200 g) and 3 wt% of p-toluenesulfonic acid (based on the total mass of the raw materials) were added to a 100 ml three-necked flask, the temperature was raised to 80°C, and the mixture was reacted for 4 h under stirring. After the reaction, 3 wt.% of NaOH solution was added to remove the unreacted guaiacol, the organic phase was collected, and the mixture was washed with deionized water for 4 times. The organic phase was collected and the water was removed by rotary evaporation to obtain plant oil-based polyphenols (cottonseed oil-based polyphenols).
[0053] According to the formula of TPU-3 shown in Table 1, the synthesized vegetable oil-based polyphenol, polyether 4110 and additives were mixed evenly, stirred with isocyanate for 20s, the speed was 2200r / min, poured into a mold, and aged at 60℃ for 24h to obtain cottonseed oil-based polyurethane foam. The prepared tung oil-based polyurethane foam was broken into 30-300 mesh powders by a high-speed multifunctional pulverizer, the pulverization power and time were 1200W and 3min respectively, and then the powder was molded into a complete cottonseed oil-based polyurethane elastomer by a manual flat vulcanizer, and the compression conditions were 120℃, 15MPa, and 20min, thereby realizing the recyclable utilization of cottonseed oil-based polyurethane foam.
[0054] Example 7
[0055] Rice bran oil (100 g), guaiacol (200 g) and 3 wt% of p-toluenesulfonic acid (based on the total mass of the raw materials) were added into a 100 ml three-necked flask, the temperature was raised to 80°C, and the mixture was reacted for 4 h under stirring. After the reaction, 3 wt.% of NaOH solution was added to remove the unreacted guaiacol, the organic phase was collected, and the mixture was washed with deionized water for 2 to 4 times. The organic phase was collected and the water was removed by rotary evaporation to obtain plant oil-based polyphenols (rice bran oil-based polyphenols).
[0056] According to the formula of TPU-3 shown in Table 1, the synthesized vegetable oil-based polyphenol, polyether 4110 and additives were mixed evenly, stirred with isocyanate for 20s, the speed was 2500r / min, poured into a mold, and aged at 60℃ for 24h to obtain rice bran oil-based polyurethane foam. The prepared tung oil-based polyurethane foam was broken into 30-300 mesh powders by a high-speed multifunctional pulverizer, the pulverization power and time were 1200W and 3min respectively, and then the powder was molded into a complete rice bran oil-based polyurethane elastomer by a manual flat vulcanizer, and the compression conditions were 120℃, 15MPa, and 20min, thereby realizing the recyclable utilization of rice bran oil-based polyurethane foam.
[0057] The tung oil-based polyphenols obtained in Example 1 were tested as follows:
[0058] Infrared spectrum test: The test was conducted using the American Nicolet IS10 FT-IR instrument. The results are shown in Figure 2 .
[0059] Depend on Figure 2 It can be seen that tung oil-based polyphenols at 3104 cm -1 (=CH stretching), 992 cm -1 (=CH bend) and 1643cm -1The absorption characteristic of tung oil does not appear at (C=C stretching), indicating that the C=C double bond in tung oil has disappeared. A new absorption peak appears at about 3388 cm -1 and 1227cm -1 These are attributed to the stretching and bending vibrations of the phenolic hydroxyl groups, respectively. -1 and 1500cm -1 The absorption peak at represents the vibration of the C=C bond of the benzene ring. The infrared spectrum results show that guaiacol has been successfully grafted onto the alkyl chain of tung oil through the Friedel-Crafts reaction.
[0060] Nuclear magnetic resonance hydrogen spectrum test: The test was carried out using a German Bruker ARX300 spectrometer (BrukerInstrument Crop, Germany), CDCl 3 As solvent, the results are shown in Figure 3 .
[0061] Depend on Figure 3 It can be seen that the chemical shift of the proton of the conjugated triene bond of tung oil (-CH=CH-CH=CH-CH=CH-) appears near 5.36~6.38 ppm, while the chemical shift of the -CH=CH- proton in tung oil-based polyphenols is found to shift to low frequencies, proving that the C=C double bond in the tung oil molecule disappears. In addition, the newly appeared multiple peaks at 6.75~7.25 ppm correspond to the chemical shift of H on the benzene ring. The results of H NMR spectroscopy show that guaiacol was successfully grafted onto the alkyl chain of tung oil.
[0062] UV spectrum test: The test was conducted using a Japanese Shimadzu RF-6000 fluorescence spectrophotometer. The results are shown in Figure 4 .
[0063] Depend on Figure 4 It can be seen that the absorption peaks at 260nm, 270nm and 281nm are attributed to the three conjugated double bonds of tung oil. The absorption peaks at 203nm, 223nm and 278nm are attributed to the E and B bands of the aromatic ring in guaiacol. For tung oil-based polyphenols, the absorption peaks at 204nm and 284nm are related to the B and E bands of the aromatic ring, and red-shift occurs due to the Friedel-Crafts alkylation reaction, while the absorption peak at 234nm is attributed to the k band caused by the π=π electron transition in the double bond of tung oil-based polyphenols. The results of UV spectroscopy test show that tung oil and guaiacol were successfully prepared from tung oil-based polyphenols through Friedel-Crafts reaction.
[0064] The polyurethane foams obtained in Example 1 according to different ratios of tung oil-based polyphenol and polyether 4110 were tested for apparent density and compression performance respectively: the test was carried out using standards GB / T6343-2009 and GB / T8813-2008, and the results are shown in Figure 5 .
[0065] Depend on Figure 5 It can be seen that with the gradual increase in the addition amount of tung oil-based polyphenols, the compressive strength of tung oil-based polyurethane foams first increases and then decreases, which indicates that an appropriate amount of vegetable oil-based polyphenols can improve the apparent density and mechanical strength of polyurethane foams; when the tung oil-based polyphenols are excessive, since the average functionality of tung oil-based polyphenols is lower than that of commercially available polyether polyols, the cross-linking degree of the polyurethane foam system is reduced, which in turn reduces the apparent density and mechanical strength of the polyurethane foam.
[0066] The polyurethane elastomers obtained by recycling different polyurethane foams in Example 1 were tested for tensile properties respectively: the test was carried out using standard ASTM D638, and the results are shown in Figure 7 .
[0067] Depend on Figure 7 It can be seen that the tung oil-based polyurethane elastomer recycled by molding exhibits good tensile properties. When TPU-3 is molded into an elastomer, the tensile strength is 19.8 MPa.
Claims
1. A method for preparing recyclable polyurethane foam using plant oil-based polyphenols, characterized in that: At room temperature, vegetable oil-based polyphenols are mixed with isocyanates and additives for reaction, poured into a mold, and cured at a certain temperature to obtain a recyclable polyurethane foam; the additives include a foaming agent, a stabilizer, and a catalyst; The vegetable oil-based polyphenol is prepared by the following method: the vegetable oil and the phenolic compound are reacted at 70-90° C. for 3-5 hours under the action of a catalyst, and the vegetable oil-based polyphenol is obtained by purification; The phenolic compound is guaiacol; the vegetable oil is one or more of tung oil, castor oil, soybean oil, palm oil, rubber seed oil, cottonseed oil, and rice bran oil; The catalyst is one or more of p-toluenesulfonic acid, tetrafluoroboric acid and phosphotungstic acid, and the amount of the catalyst accounts for 0.5-3% of the total mass of the vegetable oil and the phenolic compound.
2. A method for preparing recyclable polyurethane foam using plant oil-based polyphenols according to claim 1, characterized in that: The mass ratio of the vegetable oil to the phenolic compound is 1:(1-2).
3. The method for preparing recyclable polyurethane foam using plant oil-based polyphenols according to claim 1, characterized in that: The raw material components include, by weight, 100 parts of vegetable oil-based polyphenol, 120 parts of isocyanate, 3-4 parts of stabilizer, 0.2-0.6 parts of amine catalyst, and 5-10 parts of foaming agent.
4. The method for preparing recyclable polyurethane foam using plant oil-based polyphenols according to claim 1, characterized in that: The catalyst is N,N-dimethylcyclohexylamine; the foaming agent is one or more of HFC-141b, cyclopentane and HFC-365mfc; and the stabilizer is a silicon-type foam stabilizer.
5. The method for preparing recyclable polyurethane foam using plant oil-based polyphenols according to claim 1, characterized in that: The isocyanate is one or more of toluene diisocyanate, xylene diisocyanate, and polymethyl polyisocyanate.