A kind of fatigue-resistant composite metal material and preparation method thereof
By adding specific elements and self-made refining agents to injection mold materials, and using vacuum suspension melting and forging processes, the problems of thermal fatigue and insufficient thermal conductivity of traditional mold materials are solved, and the material is lightweight, has good thermal conductivity and has anti-fatigue properties. improvement.
Patent Information
- Application Number
- CN202310009520.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-04
AI Technical Summary
Traditional injection mold materials are prone to thermal fatigue cracks during repeated heating and cooling, which affects the surface quality and production efficiency of the product. It is also difficult to load, disassemble and repair, and has poor thermal conductivity.
An anti-fatigue composite metal material is used. Its chemical composition includes Zn, Mg, Cu, Zr, Ta, Y and other elements. It is prepared through vacuum suspension smelting and forging processes. A self-made refining agent is added to improve the purity and density of the material. Reduce hydrogen content and needle-like pores and enhance anti-fatigue properties.
The material is lightweight and has good thermal conductivity. It is suitable for rapid prototyping and loading and unloading. It significantly improves fatigue resistance, reduces the occurrence and expansion of cracks, and improves the service life and production efficiency of the mold.
Smart Images

Figure BDA0004037416550000081 
Figure BDA0004037416550000082 
Figure BDA0004037416550000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mold materials, and in particular, relates to an anti-fatigue composite metal material and a preparation method thereof. Background Art
[0002] Plastic molds are important tooling for molding plastic products. The quality of the mold directly affects the pressure processing process, the precision output of the product and the production cost. The quality and service life of the mold are mainly affected by the mold material in addition to reasonable structural design and processing accuracy.
[0003] Traditional injection molds are mainly made of mold steel, which is heavy and difficult to load, unload and repair during production. In addition, the thermal conductivity of mold steel is poor. The temperature of the plastic melt in the injection mold cavity is generally around 200°C, while the temperature of the plastic melt after cooling and hardening is only around 50°C, resulting in low production efficiency. With the development of alloy materials, traditional injection mold steels are gradually replaced by aluminum alloy molds. However, repeated heating and cooling of the mold cavity surface will cause thermal fatigue crack sources to initiate at stress concentration points. With the pulsating tensile stress on the cavity surface, the thermal fatigue cracks will expand in the depth direction, affecting the surface quality of the product. The present invention aims to develop an aluminum alloy fatigue-resistant alloy material. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide an anti-fatigue composite metal material and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A fatigue-resistant composite metal material, the chemical composition of which, by weight percentage, includes:
[0007] Zn: 8.1-8.7wt%, Mg: 2.0-2.5wt%, Cu: 1.7-2.2wt%, Zr: 0.14-0.19wt%, Ta: 0.02-0.03wt%, Y: 0.08-0.1wt%, the balance is Al and unavoidable impurities;
[0008] The preparation method thereof comprises the following steps:
[0009] Step S1: adding an aluminum ingot to a vacuum suspension melting furnace and then washing the furnace, setting the melting temperature to 750-780°C, completely melting the aluminum ingot, then adding Mg-Al master alloy and Zr-Al master alloy to keep them warm and melt, and performing a slag removal, controlling the furnace temperature to 700-720°C, adding Zn powder and Cu powder for melting, and then using a bell jar to press into a refining agent for deoxidation and dehydrogenation for several times, performing a secondary slag removal, unloading from the furnace, and casting to form an alloy ingot;
[0010] Furthermore, the vacuum suspension melting furnace cleaning operation specifically includes: evacuating the furnace to below 0.5kPa, introducing high-purity nitrogen until a stable airflow is discharged, evacuating the furnace to below 2kPa again, and introducing argon to a constant pressure to avoid oxidation during the long-term smelting process of the aluminum ingot, thereby ensuring the purity of the original aluminum liquid.
[0011] Step S2: placing the alloy ingot in a vacuum furnace, keeping the temperature at 280-300° C. for 2-2.5 hours, then heating it to 400-420° C. for 3-4 hours, and then continuing to heat it to 455-470° C. for 18-20 hours, homogenizing the alloy ingot to make a homogenized casting;
[0012] Step S3: heating the homogenized casting to 430° C., placing it in a forging press for extrusion, controlling the temperature of the extrusion die to be 420-430° C., and the extrusion ratio to be 9-11, extrusion-forging the homogenized casting to produce a forged part;
[0013] Step S4: heating the forged part to 460-480° C. and keeping the temperature for 1-1.2 hours, placing the forged part in cooling water for quenching, and subjecting the forged part to solid solution quenching treatment to produce a solid solution quenched part;
[0014] Step S5: heating the solution quenched part to 120° C., keeping the temperature for 24 hours, cooling it naturally to room temperature, and subjecting the solution quenched part to aging treatment to produce a fatigue-resistant composite metal material.
[0015] The refining agent is prepared by the following method:
[0016] Step A1: calcining the zeolite powder in a muffle furnace at 400° C. for 3 h, discharging the zeolite powder into a weakly acidic sodium chloride solution for quenching and allowing the solution to stand for 2-3 days, then filtering the solution, washing the filter cake, and drying the filter cake to prepare a porous carrier;
[0017] Furthermore, the fineness of the zeolite powder is 200-325 meshes, the concentration of the weakly acidic sodium chloride solution is 5-8%, the pH value is 5.5-6.0, and the solid-liquid ratio of the zeolite powder to the weakly acidic sodium chloride solution is 1:18-23.
[0018] Step A2: Dissolve hexachloroethane and ethanol solution, add porous carrier to mix, stir and soak at room temperature, then introduce nitrogen protection, add nano tantalum powder and high purity yttrium powder for ultrasonic dispersion, then reduce pressure and rotary evaporate, and take the rotary evaporated product to prepare the refining agent.
[0019] Furthermore, the usage ratio of the porous carrier, hexachloroethane, nano tantalum powder and high-purity yttrium powder is 10g:3.8g:0.55-0.62g:1.7-1.9g.
[0020] Beneficial effects of the present invention:
[0021] 1. The present invention manufactures an aluminum-based alloy material through reasonable formula design and process selection. Compared with traditional mold steel, the aluminum-based alloy material has the characteristics of light weight and good thermal conductivity. It is applied to injection molds, which is beneficial to the loading and unloading of molds and rapid molding.
[0022] 2. The present invention adds a self-made refining agent during the smelting process, wherein the zeolite powder is used as a carrier, and the crystal water is fully removed by roasting and the impurities in the pores are burned off. In a weakly acidic solution environment, the sodium ions are replaced with the calcium in the zeolite powder, so that the pores of the zeolite powder are enlarged, and the zeolite powder has a good adsorption loading capacity. Then, an ethanol solution is used as a dispersant to load hexachloroethane, nano tantalum powder and high-purity yttrium powder, wherein the hexachloroethane is vaporized during the refining process, which is conducive to the floating removal of the zeolite carrier, the removal of free gas in the alloy liquid, and the yttrium and oxygen are reacted. The strong bonding effect can take away the oxygen in the aluminum oxide in the melt, which plays a role of deoxidation on the one hand, and on the other hand, yttrium takes away oxygen to form a high-melting-point complex. As the crystallization core of aluminum, it has a metamorphic effect on aluminum oxide inclusions, greatly reducing cracks caused by inclusions and crack propagation; Tantalum has a strong hydrogen absorption ability at around 700°C, which effectively reduces the hydrogen content in aluminum-based materials, reduces needle-shaped pores, greatly improves the purity and density of the matrix, and can effectively resist fatigue stress, thereby showing good anti-fatigue properties. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The present invention is based on the existing high-strength aluminum mold material and designs the alloy material. The specific target composition of the alloy material is designed as follows: Zn: 8.4wt%, Mg: 2.2wt%, Cu: 1.8wt%, Zr: 1.6wt%, and the balance is Al and inevitable impurities. According to production experience, the burnout rate of Al is set to 4.2%, the burnout rates of Zn and Mg are 8.5%, and the burnout rates of Cu and Zr are 0.4%.
[0025] Example 1
[0026] This embodiment prepares an anti-fatigue composite metal material, and the specific implementation process is as follows:
[0027] 1. Preparation of refining agent
[0028] a1, taking zeolite powder (calibrated fineness is 200 mesh) and placing it in a muffle furnace at 400 ° C for 3h, taking sodium chloride dissolved in water to prepare a dilute solution with a concentration of 5%, adding hydrochloric acid to adjust the pH value to 5.5, preparing a weakly acidic sodium chloride solution as a quenching liquid, adding the calcined zeolite powder to the weakly acidic sodium chloride solution at a solid-liquid ratio of 1:18, quenching and standing for 2d, the zeolite powder is fully calcined to remove crystal water and burn out impurities in the pores, in the weakly acidic solution environment, sodium ions are replaced with calcium in the zeolite powder, so that the pores of the zeolite powder are enlarged, and the filter cake is filtered out after soaking, washed with water, and placed in a drying oven to dry to constant weight to prepare a porous carrier;
[0029] a2. Hexachloroethane and 50% ethanol solution were mixed at a solid-liquid ratio of 1:40, and mechanically stirred at 120 rpm until completely dissolved. A porous carrier was added and stirred and soaked at room temperature for 4 hours. After that, nitrogen was introduced to expel the air. Nano tantalum powder and high-purity yttrium powder were added, and ultrasonic dispersion treatment was performed at 40 kHz for 30 minutes. The amount ratio of porous carrier, hexachloroethane, nano tantalum powder and high-purity yttrium powder was 10 g: 3.8 g: 0.55 g: 1.9 g. The dispersion was decompressed to 1 kPa, heated to 60°C and evaporated until no water was discharged to prepare a refining agent.
[0030] 2. Preparation of composite metal materials
[0031] s1. Melting: Take the aluminum ingot and add it into the vacuum suspension melting furnace. Evacuate the furnace to below 0.5kPa, introduce high-purity nitrogen until a stable airflow is discharged, evacuate the furnace to below 2kPa again, introduce argon to a constant pressure, wash the vacuum suspension melting furnace to avoid oxidation during the long-term melting of the aluminum ingot and ensure the purity of the original aluminum liquid. Set the melting temperature to 780℃, melt for 15min, completely melt the aluminum ingot, and add Mg-Al master alloy (Al-5 0Mg) and Zr-Al (Al-4Zr) master alloy, heat-smelting for 6 minutes, perform a slag removal, control the furnace temperature to 720°C after slag removal, add Zn powder and Cu powder for smelting for 10 minutes, take 1.0wt% of refining agent of alloy liquid, use bell jar to press 70% of refining agent first, heat-smelting for 3 minutes, then press the remaining refining agent again, heat-smelting for 5 minutes, perform a secondary slag removal, take the alloy liquid out of the furnace at 750°C, cast, and make alloy ingot;
[0032] s2. Homogenization: Place the alloy ingot in a vacuum furnace, maintain the vacuum degree at 3 kPa, heat it to 300 °C and keep it for 2 hours, then slowly heat it to 420 °C at 8 °C / min and keep it for 3 hours, then continue to heat it to 470 °C and keep it for 18 hours, homogenize the alloy ingot, and make a homogenized casting;
[0033] s3. Extrusion forging: The homogenized casting is heated to 430°C and placed in a forging press for extrusion. The extrusion die is pre-heated to 430°C and the extrusion ratio is controlled to be 11. The homogenized casting is subjected to extrusion forging to form a forged part.
[0034] s4. Heat the forging to 480°C and keep it for 1 hour, control the furnace temperature to be no less than 450°C, place it in cooling water for quenching, perform solid solution quenching on the forging to make a solid solution quenched part;
[0035] s5. Heat the solution quenched parts to 120°C, keep them warm for 24 hours, cool them naturally to room temperature, and perform aging treatment on the solution quenched parts to produce fatigue-resistant composite metal materials.
[0036] Example 2
[0037] This embodiment prepares an anti-fatigue composite metal material, and the specific implementation process is as follows:
[0038] 1. Preparation of refining agent
[0039] a1. Take zeolite powder (with a nominal fineness of 325 mesh) and place it in a muffle furnace and roast it at 400° C. for 3 hours. At the same time, take sodium chloride and dissolve it in water to prepare a dilute solution with a concentration of 5%. Add hydrochloric acid to adjust the pH value to 6.0 to prepare a weakly acidic sodium chloride solution as a quenching liquid. The calcined zeolite powder is added to the weakly acidic sodium chloride solution at a solid-liquid ratio of 1:23, quenched, and allowed to stand and soak for 3 days. After soaking, filter out the filter cake, add water to wash, and place it in a drying oven to dry to constant weight to prepare a porous carrier;
[0040] a2. Hexachloroethane and 50% ethanol solution were mixed at a solid-liquid ratio of 1:40, and mechanically stirred at 120 rpm until completely dissolved. A porous carrier was added and stirred and soaked at room temperature for 5 hours. After that, nitrogen was introduced to expel the air. Nano tantalum powder and high-purity yttrium powder were added, and ultrasonic dispersion treatment was performed at 40 kHz for 50 minutes. The amount ratio of porous carrier, hexachloroethane, nano tantalum powder and high-purity yttrium powder was 10 g: 3.8 g: 0.62 g: 1.7 g. The dispersion was decompressed to 1 kPa, heated to 60°C and evaporated until no water was discharged to prepare a refining agent.
[0041] 2. Preparation of composite metal materials
[0042] s1. Melting: take an aluminum ingot and add it to a vacuum suspension melting furnace, evacuate the furnace to below 0.5 kPa, introduce high-purity nitrogen until a stable airflow is discharged, evacuate the furnace to below 2 kPa again, introduce argon to a constant pressure, wash the vacuum suspension melting furnace, set the melting temperature to 750°C, melt for 20 minutes, completely melt the aluminum ingot, add Mg-Al master alloy and Zr-Al master alloy, keep warm and melt for 8 minutes, perform a slag removal, control the furnace temperature to 700°C after slag removal, add Zn powder and Cu powder and melt for 12 minutes, take 0.8wt% of the alloy liquid refining agent, use a bell jar to press in 70% of the refining agent first, keep warm and melt for 5 minutes, then press in the remaining refining agent again, keep warm for 8 minutes, perform a second slag removal, the alloy liquid is discharged from the furnace at 740°C, cast, and made into an alloy ingot;
[0043] s2. Homogenization: Place the alloy ingot in a vacuum furnace, maintain the vacuum degree at 3 kPa, heat it to 280 °C and keep it for 2.5 hours, then slowly heat it to 400 °C at 8 °C / min and keep it for 4 hours, then continue to heat it to 455 °C and keep it for 20 hours, homogenize the alloy ingot, and make a homogenized casting;
[0044] s3. Extrusion forging: The homogenized casting is heated to 430°C and placed in a forging press for extrusion. The extrusion die is pre-heated to 420°C and the extrusion ratio is controlled to 9. The homogenized casting is subjected to extrusion forging to form a forged part.
[0045] s4. Raise the temperature of the forged parts to 460°C and keep it for 1.2 hours. Control the furnace temperature to be no less than 450°C. Quench the forged parts in cooling water and perform solid solution quenching treatment on the forged parts to make solid solution quenched parts.
[0046] s5. Heat the solution quenched parts to 120°C, keep them warm for 24 hours, cool them naturally to room temperature, and perform aging treatment on the solution quenched parts to produce fatigue-resistant composite metal materials.
[0047] Example 3
[0048] This embodiment prepares an anti-fatigue composite metal material, and the specific implementation process is as follows:
[0049] 1. Preparation of refining agent
[0050] a1. Take zeolite powder (with a nominal fineness of 325 mesh) and place it in a muffle furnace and roast it at 400° C. for 3 hours. At the same time, take sodium chloride and dissolve it in water to prepare a dilute solution with a concentration of 7%. Add hydrochloric acid to adjust the pH value to 5.5 to prepare a weakly acidic sodium chloride solution as a quenching liquid. The calcined zeolite powder is added to the weakly acidic sodium chloride solution at a solid-liquid ratio of 1:20, quenched, and allowed to stand and soak for 3 days. After soaking, filter out the filter cake, add water to wash, and place it in a drying oven to dry to constant weight to prepare a porous carrier;
[0051] a2. Hexachloroethane and 50% ethanol solution were mixed at a solid-liquid ratio of 1:38, and mechanically stirred at 120 rpm until completely dissolved. A porous carrier was added and stirred and soaked at room temperature for 5 hours. After that, nitrogen was introduced to expel the air. Nano tantalum powder and high-purity yttrium powder were added, and ultrasonic dispersion treatment was performed at 40 kHz for 40 minutes. The amount ratio of porous carrier, hexachloroethane, nano tantalum powder and high-purity yttrium powder was 10 g: 3.8 g: 0.58 g: 1.8 g. The dispersion was decompressed to 1 kPa, heated to 60°C and evaporated until no water was discharged to prepare a refining agent.
[0052] 2. Preparation of composite metal materials
[0053] s1. Melting: take an aluminum ingot and add it to a vacuum suspension melting furnace, evacuate the furnace to below 0.5 kPa, introduce high-purity nitrogen until a stable airflow is discharged, evacuate the furnace to below 2 kPa again, introduce argon to a constant pressure, wash the vacuum suspension melting furnace, set the melting temperature to 770°C, melt for 18 minutes, completely melt the aluminum ingot, add Mg-Al master alloy and Zr-Al master alloy, keep warm and melt for 7 minutes, perform a slag removal, control the furnace temperature to 710°C after slag removal, add Zn powder and Cu powder and melt for 12 minutes, take 0.9wt% of the alloy liquid refining agent, use a bell jar to press in 70% of the refining agent first, keep warm and melt for 4 minutes, then press in the remaining refining agent again, keep warm for 7 minutes, perform a second slag removal, the alloy liquid is discharged from the furnace at 740°C, cast, and made into an alloy ingot;
[0054] s2. Homogenization: Place the alloy ingot in a vacuum furnace, maintain the vacuum degree at 3 kPa, heat it to 300 °C and keep it for 2.2 hours, then slowly heat it to 410 °C at 8 °C / min and keep it for 3.6 hours, then continue to heat it to 465 °C and keep it for 19 hours, homogenize the alloy ingot, and make a homogenized casting;
[0055] s3. Extrusion forging: The homogenized casting is heated to 430°C and placed in a forging press for extrusion. The extrusion die is pre-heated to 430°C and the extrusion ratio is controlled to be 10. The homogenized casting is subjected to extrusion forging to form a forged part.
[0056] s4. Heat the forging to 470°C and keep it for 1.1h, control the furnace temperature to be not less than 450°C, place it in cooling water for quenching, perform solid solution quenching on the forging to make a solid solution quenched part;
[0057] s5. Heat the solution quenched parts to 120°C, keep them warm for 24 hours, cool them naturally to room temperature, and perform aging treatment on the solution quenched parts to produce fatigue-resistant composite metal materials.
[0058] The composite metal materials prepared in Examples 1 to 3 were sampled and the chemical composition of the samples was tested. The specific test data are shown in Table 1:
[0059] Table 1
[0060]
[0061] It can be seen from the data in Table 1 that the chemical composition of the composite metal material prepared by the present invention is Zn: 8.1-8.7wt%, Mg: 2.0-2.5wt%, Cu: 1.7-2.2wt%, Zr: 0.14-0.19wt%, Ta: 0.02-0.03wt%, Y: 0.08-0.1wt%, and the remainder is Al and unavoidable impurities.
[0062] Comparative Example
[0063] This comparative example is the existing 7055 high-strength aluminum alloy mold material.
[0064] The composite metal materials prepared in Examples 1 to 3 and the aluminum alloy materials provided in the comparative example were sampled and subjected to thermal fatigue tests using the Uddeholm self-restraint method. The test process is as follows:
[0065] In one cycle, the sample is first quickly heated to 300°C by the induction coil, and then cooled to below 80°C by spraying water for thermal fatigue cycle test. After 50,000 cycles of thermal fatigue test, the fatigue crack parameter of the test sample takes the maximum value. The specific test data are shown in Table 2:
[0066] Table 2
[0067]
[0068]
[0069] It can be seen from the data in Table 2 that after 50,000 fatigue tests, the maximum crack depth of the composite metal material prepared by the present invention is 26-35 μm, the maximum crack width is 12-19 μm, and the crack state is discontinuous cracking, which is a typical primary fatigue crack. Compared with the existing 7055 high-strength aluminum alloy mold material, it shows good anti-fatigue properties.
[0070] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0071] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing an anti-fatigue composite metal material, characterized in that: The fatigue-resistant composite metal material is made by melting aluminum ingots, Mg-Al master alloys, Zr-Al master alloys, Zn powders and Cu powders as raw materials and casting them into alloy ingots, and then performing homogenization treatment, extrusion forging, solid solution quenching treatment and aging treatment in sequence; The chemical composition of the fatigue-resistant composite metal material is as follows by weight percentage: Zn: 8.1-8.7wt%, Mg: 2.0-2.5wt%, Cu: 1.7-2.2wt%, Zr: 0.14-0.19wt%, Ta: 0.02-0.03wt%, Y: 0.08-0.1wt%, and the balance is Al and unavoidable impurities. Refining agents are added during the smelting process to remove oxygen and dehydrogenate. The refining agent is prepared by the following method: Step A1: calcining zeolite powder in a muffle furnace at 400° C. for 3 h, discharging the zeolite powder into a weakly acidic sodium chloride solution for quenching and standing for 2-3 d, then filtering, washing and drying the filter cake to prepare a porous carrier, wherein the zeolite powder has a fineness of 200-325 mesh, sodium chloride is prepared into a dilute solution, and the pH is adjusted to weak acidity with hydrochloric acid, the concentration of the weakly acidic sodium chloride solution is 5-8%, the pH value is 5.5-6.0, and the solid-liquid ratio of the zeolite powder to the weakly acidic sodium chloride solution is 1:18-23; Step A2: dissolving hexachloroethane and ethanol solution, adding a porous carrier to the mixture, stirring and soaking at room temperature, then introducing nitrogen protection, adding nano tantalum powder and high-purity yttrium powder for ultrasonic dispersion, and then vacuum rotary evaporation, taking the rotary evaporation product to prepare a refining agent, wherein the amount ratio of the porous carrier, hexachloroethane, nano tantalum powder and high-purity yttrium powder is 10g:3.8g:0.55-0.62g:1.7-1.9g; The refining agent is added during the smelting process, and the furnace temperature is 700-720°C when added.
2. The method for preparing a fatigue-resistant composite metal material according to claim 1, characterized in that: The specific smelting method is as follows: adding the aluminum ingot to the vacuum suspension smelting furnace and then washing the furnace, setting the smelting temperature to 750-780°C, completely melting the aluminum ingot, adding Mg-Al master alloy and Zr-Al master alloy to keep warm and melt and perform a slag removal, controlling the furnace temperature to 700-720°C, adding Zn powder and Cu powder for smelting, and then using a bell jar to press in refining agents for deoxidation and dehydrogenation for several times, performing a secondary slag removal, unloading from the furnace, and casting to form an alloy ingot.
3. The method for preparing a fatigue-resistant composite metal material according to claim 2, characterized in that: The specific method of homogenization treatment is: place the alloy ingot in a vacuum furnace, keep it at 280-300℃ for 2-2.5h, then heat it to 400-420℃ for 3-4h, and then continue to heat it to 455-470℃ for 18-20h to make a homogenized casting.
4. The method for preparing a fatigue-resistant composite metal material according to claim 3, characterized in that: The homogenized casting is heated to 430°C and placed in a forging press for extrusion. The temperature of the extrusion die is controlled at 420-430°C and the extrusion ratio is 9-11 to produce a forged part.
5. The method for preparing a fatigue-resistant composite metal material according to claim 4, characterized in that: The forgings are heated to 460-480°C and kept at this temperature for 1-1.2 hours, then quenched in cooling water to form solution-quenched parts.
6. The method for preparing a fatigue-resistant composite metal material according to claim 5, characterized in that: The solution quenched parts are heated to 120°C, kept at this temperature for 24 hours, and naturally cooled to room temperature to produce fatigue-resistant composite metal materials.
Citation Information
Patent Citations
Hot rolled aluminum-zinc alloy plate and preparation method thereof
CN103710595A
Super-strength and high-ductility Al-Zn-Mg-Cu series aluminum alloy and preparation process thereof
CN110042287A
High-strength closed-cell foamed aluminum alloy and preparation method thereof
CN110468313A
Production process of die-casting aluminum alloy for high-toughness light-weight structural part
CN114892031A