A hydrophobically modified zeolite molecular sieve and its preparation method and application

By coating the surface of the zeolite molecular sieve with a fluorocarbon layer, the problem of reduced CO2 adsorption performance of the zeolite molecular sieve in a wet environment is solved, efficient and economical hydrophobic modification is achieved, and the repeated stability and regeneration ability of the material are improved, making it suitable for industrialization. application.

CN116237011BActive Publication Date: 2024-10-11TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310361471.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-11
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

The adsorption performance of existing zeolite molecular sieves for CO2 decreases in wet environments, and the hydrophobic modification process is complex, long-term, and costly, and the problems of repeatability and regeneration energy consumption have not been effectively solved.

Method used

By coating the surface of the zeolite molecular sieve with a uniform and stable fluorocarbon hydrophobic layer, and using simple impregnation and carbonization processes, a hydrophobically modified zeolite molecular sieve is prepared, which is suitable for industrial large-scale production.

Benefits of technology

It improves the CO2 adsorption capacity and selectivity of zeolite molecular sieves in wet environments. The material maintains good adsorption and separation capabilities at high temperatures and is easy to regenerate. It is suitable for hydrophobic modification of various zeolite molecular sieves.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116237011B_ABST
    Figure CN116237011B_ABST
Patent Text Reader

Abstract

The present invention is a hydrophobically modified zeolite molecular sieve and its preparation method and application. The composition of the molecular sieve includes a zeolite molecular sieve and a fluorinated carbon layer coated thereon; the thickness of the fluorinated carbon layer is 2 to 6 microns; the mass of the fluorinated carbon is 5% to 60% of the mass of the zeolite molecular sieve; during the preparation, a layer of organic polymer containing fluorine functional groups is coated on the surface of the zeolite molecular sieve by simple impregnation and carbonization, and after calcination, a uniform and stable fluorinated carbon hydrophobic layer is obtained. The preparation method of the present invention is simple, short in cycle, and high in output, and is suitable for large-scale industrial development; compared with other hydrophobically modified molecular sieves, the fluorinated carbon coated zeolite molecular sieve has the advantages of easy regeneration and good repeated stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a porous solid adsorbent for gas adsorption separation, and more specifically, to a method for preparing a porous solid adsorbent that can be repeatedly and efficiently used in a humid environment, and belongs to the field of porous composite carbon materials.

[0002] The present invention relates to the technical field of molecular sieves, and in particular to a hydrophobically modified molecular sieve and a preparation method and application thereof. Background Art

[0003] In recent years, carbon capture and storage (sequestration) (CCS) has been considered as a potential way to allow the continued use of fossil fuel power stations while preventing carbon dioxide emissions into the atmosphere. Gas, coal (and biomass) fired power stations are more responsive to changes in demand than many other sources of electricity production, so it is important to have them as an option in the energy mix. Typical flue gases from coal-fired boilers contain carbon dioxide, water, oxygen, nitrogen, etc. Capturing carbon from flue gases has become an important technical challenge at present.

[0004] Adsorption separation is a mature process in the current chemical industry, and is widely used due to its high selectivity, green cleanliness, and renewability. The most critical factor affecting adsorption separation is the adsorbent. Zeolite molecular sieves have been widely used in adsorption separation, catalysis, and other fields due to their high specific surface area and unique pore structure. Zeolite molecular sieves not only have high adsorption performance for CO2 at normal pressure, as well as high thermal stability and good adjustability, but also have a high CO2 adsorption capacity at low pressure. However, most zeolite molecular sieves are extremely sensitive to the presence of water. There is a serious competitive relationship between water molecules and CO2 capture, which deactivates some pores and cannot capture CO2. This will cause the working capacity and stability of zeolite molecular sieves to be seriously reduced in actual post-combustion flue gas capture.

[0005] The methods currently reported include a combination of hydrothermal generation and acid extraction, silicon tetrachloride method, ammonium hexafluorosilicate method, CVD method, etc., which reduce the content of crystalline aluminum to eliminate polar ions in the framework structure, thereby achieving a hydrophobic effect. CN112390270A, CN115445582A, CN114570328A, CN102992341B and CN115228431A all disclose methods for hydrophobic modification of zeolite molecular sieves, but there are problems such as complex process, long cycle, high cost, etc. in the process of hydrophobic modification, and few inventions mention the repeated stability of materials and the problem of regeneration energy consumption.

[0006] Therefore, there is an urgent need to develop a modified zeolite molecular sieve that is easy to regenerate, has good repeated stability, has a high adsorption capacity and selectivity for CO2 in a high humidity environment, and a simple, economical and rapid method for hydrophobic modification of zeolite molecular sieves. Summary of the invention

[0007] The purpose of the present invention is to provide a hydrophobically modified zeolite molecular sieve and its preparation method and application in view of the deficiencies in the current technology. The present invention uses simple impregnation and carbonization to coat a uniform and stable fluorinated carbon hydrophobic layer on the surface of the zeolite molecular sieve. The preparation method is simple, the cycle is short, and the output is large. It is suitable for the hydrophobic modification treatment of almost all zeolite molecular sieves. It is suitable for large-scale industrial development; compared with other hydrophobically modified molecular sieves, the fluorinated carbon coated zeolite molecular sieve has the advantages of easy regeneration and good repeated stability.

[0008] The purpose of the present invention is achieved by the following technical solutions:

[0009] A hydrophobic modified zeolite molecular sieve (ZSM@MPC for short) comprises a zeolite molecular sieve and a fluorinated carbon layer coated thereon; the thickness of the fluorinated carbon layer is 2 to 6 microns; the mass of the fluorinated carbon is 5% to 60% of the mass of the zeolite molecular sieve.

[0010] The zeolite molecular sieve is specifically an X-type molecular sieve, a Y-type molecular sieve, an MFI-type molecular sieve, an A-type molecular sieve or a B-type molecular sieve.

[0011] The particle size of the zeolite molecular sieve is in the range of 2 to 5 mm;

[0012] The method for preparing the hydrophobically modified zeolite molecular sieve comprises the following steps:

[0013] (1) Keep the zeolite molecular sieve at 200-600°C for 1-4 hours to obtain an activated molecular sieve;

[0014] (2) Immerse the activated molecular sieve in the mixed solution and stir at 20°C to 30°C for 8 to 12 hours to obtain a zeolite molecular sieve coated with a polymer containing a fluorine functional group;

[0015] The mixed solution is acetone containing an organic polymer containing a fluorine functional group, the concentration of the polymer is in the range of 5wt% to 60wt%, and 10g to 30g of molecular sieve is added to every 15g to 45g of the mixed solution;

[0016] (3) The polymer-coated zeolite molecular sieve obtained in the previous step was placed in a blast drying oven at 60°C to 100°C and dried for 4 to 8 hours;

[0017] (4) Place the dried material obtained in the previous step into a heating furnace, raise the temperature to 400-700°C under nitrogen protection, and keep the temperature constant for 3-6 hours;

[0018] (5) Cool to room temperature and discharge the material to obtain a hydrophobically modified zeolite molecular sieve.

[0019] The organic polymer containing fluorine functional groups is fluoroplastic, fluororubber and fluoro coating, specifically polytetrafluoroethylene (PTFE), soluble polytetrafluoroethylene (PFA), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE) and FKM (fluororubber).

[0020] In the step (4), the heating rate is 5 to 15°C / min.

[0021] The hydrophobically modified zeolite molecular sieve composite material is used for capturing CO2 in wet flue gas, air separation or natural gas purification.

[0022] The method of capturing CO2 from wet flue gas specifically comprises the following steps: passing the flue gas into a columnar reactor containing a hydrophobically modified zeolite molecular sieve composite material to complete the capture and separation of CO2 from the wet flue gas; wherein the components in the flue gas include CO2 (12-14 vol%), H2O (8-10 vol%) and N2 (72-77 vol%); the air velocity is 1-10 h -1 ; The temperature is 5~30℃.

[0023] The regeneration method of the hydrophobically modified zeolite molecular sieve composite material comprises the following steps:

[0024] In an atmosphere of inert gas, keep the temperature at 120-180°C for 1-3 hours, and then cool to room temperature. The inert gas is helium.

[0025] The beneficial effects of the present invention are:

[0026] The present invention is simple to operate, has no complicated procedures, does not require special equipment, is low in cost, and is suitable for industrial large-scale production; the pore structure of the modified zeolite molecular sieve does not change much, and still maintains its good pore properties, and significantly improves the material's adsorption of CO2 in the presence of water. The fluorinated carbon coating effectively blocks the zeolite molecular sieve's competitive adsorption of water, retains more active sites for adsorbing CO2, and greatly improves the adsorption of CO2 in actual flue gas after combustion. At the same time, the present invention is suitable for hydrophobic modification of a variety of commercially available zeolite molecular sieves, and has broad market prospects.

[0027] The material obtained by the present invention desorbs CO2 gas when heated at 120-160°C, is easy to regenerate, and can maintain good adsorption and separation capabilities after four consecutive cycles of regeneration. Preferably, the material 13X@PVDF (25,550) prepared by the present invention has a CO2 retention time that is more than 4 times higher than that of the original material 13X in actual wet flue gas separation, and the adsorption of water molecules is reduced by half. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a carbon element line scanning image of the cross section of 13X@PVDF (25,550) obtained in Example 1;

[0029] Figure 2 The XRD patterns of 13X and 13X@PVDF(25,550) obtained in Example 1 are shown in FIG.

[0030] Figure 3 The adsorption isotherm of CO2 of 13X@PVDF (25,550) at 273K;

[0031] Figure 4 This is a graph showing four consecutive gas adsorption and separation cycles of 13X@PVDF (25,550) obtained in Example 1 for a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v);

[0032] Figure 5 This is the gas adsorption separation experimental diagram of 13X obtained in Example 1 for a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v). DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other examples obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Embodiment 1:

[0035] A hydrophobically modified zeolite molecular sieve and a preparation method and application thereof, the steps are as follows:

[0036] (1) Weigh 20g of 13X molecular sieve, activate it at 500℃ for 2h, and then immerse it in 5g of polyvinylidene fluoride (PVDF) and 30g of acetone to form a mixed solution, stir it overnight, and then place the mixture in a forced air drying oven at 80℃ to dry it for 6h.

[0037] (2) The mixture was placed in a tubular furnace, heated to 550° C. at a heating rate of 5° C. / min in a nitrogen atmosphere, and kept at this temperature for 5 h to obtain a fluorinated carbon-coated zeolite molecular sieve 13X@PVDF (25,550).

[0038] The zeolite molecular sieve used in this embodiment is 13X molecular sieve, also called sodium X-type molecular sieve, which is an alkali metal aluminosilicate with a certain alkalinity and a chemical formula of Na2O·Al2O3·2.45SiO2·6.0H20. Zeolite 13X molecular sieve is provided by Dalian Zeer Catalytic Materials Co., Ltd., and has an average particle size of 2 to 3 mm. Since they are all known materials, different types of molecular sieves are no longer listed one by one.

[0039] Figure 1 This is a carbon element line scan image of the cross section of 13X@PVDF (25,550). As shown in the figure, the zeolite molecular sieve is coated with a uniform and thin carbon layer, and the thickness of the fluorinated carbon layer is about 4 microns.

[0040] Figure 2 The XRD spectra of 13X and 13X@PVDF(25,550) show that carbon coating does not affect the structure of zeolite. 13X@MPC(25,550) shows a sharp peak at around 6.16°, and the corresponding d spacing is about 1.4nm, which is consistent with the standard 13X zeolite. This shows that carbon atoms do not destroy the order of structural pores.

[0041] Figure 3 This is the adsorption isotherm of CO2 of 13X@PVDF (25,550) at 273K. It can be observed from the figure that the material still maintains a high adsorption capacity for CO2, and has a higher adsorption capacity in the low pressure area, indicating that the material still retains a large number of ultra-micropores after activation.

[0042] An application of a fluorinated carbon-coated zeolite molecular sieve for efficient carbon capture from wet flue gas, a solid adsorbent for separating CO2 from wet flue gas, and a breakthrough experiment designed to detect the actual adsorption and separation of the sample. The method is: at room temperature of 25°C, 4g13X@PVDF (25,550) is loaded into a quartz column with an inner diameter of 8mm, and one end of the quartz column is connected to a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) with a flow rate of 2ml / min (space velocity 2.88h -1 ), and the other end is connected to a mass spectrometer to detect the adsorption and separation of the gas. The sample column can be heated at 150℃ for 2h in a helium atmosphere to desorb and regenerate the sample CO2.

[0043] Figure 4The graph shows the 4-cycle gas adsorption separation experiment of 13X@PVDF(25,550) for mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v). It can be seen from the graph that the 13X@PVDF(25,550) material has good repeated stability for CO2 adsorption separation, and the adsorption retention time of CO2 is 4 times higher than that of the raw material 13X.

[0044] Embodiment 2:

[0045] A hydrophobically modified zeolite molecular sieve and a preparation method and application thereof, the steps are as follows:

[0046] (1) Weigh 30g of 4A molecular sieve and activate it at 400℃ for 4h, then immerse it in 3.0g of polyvinylidene fluoride (PVDF) and 40g of acetone to form a mixed solution, stir overnight, and then place the mixture in a forced air drying oven at 80℃ to dry for 6h.

[0047] (2) The mixture was placed in a tubular furnace, heated to 500° C. at a heating rate of 5° C. / min in a nitrogen atmosphere, and kept at this temperature for 5 h to obtain carbonized carbon-coated zeolite molecular sieve 4A@PVDF (10,500).

[0048] The cross-sectional carbon element line scanning image, XRD spectrum and CO2 adsorption isotherm at 273K of the obtained 4A@PVDF (10,500) are similar to those in Example 1.

[0049] An application of a fluorinated carbon-coated zeolite molecular sieve for efficient carbon capture from wet flue gas, a solid adsorbent for separating CO2 from wet flue gas, and a breakthrough experiment designed to detect the actual adsorption and separation of the sample. The method is: at room temperature of 25°C, 4g4A@PVDF (10,500) is loaded into a quartz column with an inner diameter of 8mm, and one end of the quartz column is connected to a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) with a flow rate of 2ml / min (i.e., a space velocity of 2.88h -1 ), and the other end is connected to a mass spectrometer to detect the adsorption and separation of the gas. The sample column can be heated at 150℃ for 2h in a helium atmosphere to desorb and regenerate the sample CO2.

[0050] The experimental diagram of 4A@PVDF (10,500) for 4 consecutive gas adsorption and separation cycles of the mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that of Example 1.

[0051] Embodiment 3:

[0052] A hydrophobically modified zeolite molecular sieve and a preparation method and application thereof, the steps are as follows:

[0053] (1) Weigh 10 g of ZSM-5 molecular sieve, activate it at 500°C for 2 h, and then immerse it in 3.0 g of polyvinylidene fluoride (PVDF) and 15 g of acetone to form a mixed solution, stir it overnight, and then place the mixture in a forced air drying oven at 80°C to dry it for 6 h.

[0054] (2) The mixture was placed in a tubular furnace, heated to 500°C at a heating rate of 5°C / min in a nitrogen atmosphere, and kept at this temperature for 5 h to obtain a fluorinated carbon-coated zeolite molecular sieve ZSM-5@PVDF (30,500).

[0055] The cross-sectional carbon element line scanning image, XRD spectrum and CO2 adsorption isotherm at 273K of the obtained ZSM-5@PVDF(30,500) are similar to those in Example 1.

[0056] An application of a fluorinated carbon-coated zeolite molecular sieve for efficiently capturing carbon from wet flue gas, a solid adsorbent for separating CO2 from wet flue gas, and a breakthrough experiment designed to detect the actual adsorption and separation of the sample. The method is: at room temperature of 25°C, 4g ZSM-5@PVDF (30,500) is loaded into a quartz column with an inner diameter of 8mm, and one end of the quartz column is connected to a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) with a flow rate of 2ml / min (i.e., a space velocity of 2.88h -1 ), and the other end is connected to a mass spectrometer to detect the adsorption and separation of the gas. The sample column can be heated at 150℃ for 2h in a helium atmosphere to desorb and regenerate the sample CO2.

[0057] The experimental graph of four consecutive gas adsorption and desorption cycles of ZSM-5@PVDF (30,500) for a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that in Example 1.

[0058] Embodiment 4:

[0059] A hydrophobically modified zeolite molecular sieve and a preparation method and application thereof, the steps are as follows:

[0060] (1) Weigh 20g of 10X molecular sieve and activate it at 550℃ for 2h, then immerse it in 7.0g of polyvinylidene fluoride (PVDF) and 25g of acetone to form a mixed solution, stir overnight, and then place the mixture in a forced air drying oven at 80℃ to dry for 6h.

[0061] (2) The mixture was placed in a tubular furnace, heated to 600° C. at a heating rate of 5° C. / min in a nitrogen atmosphere, and kept at this temperature for 5 h to obtain a fluorinated carbon-coated zeolite molecular sieve 10X@PVDF (35,600).

[0062] The cross-sectional carbon element line scanning image, XRD spectrum and CO2 adsorption isotherm at 273K of the obtained 10X@PVDF (35,600) are similar to those in Example 1.

[0063] An application of a fluorinated carbon-coated zeolite molecular sieve for efficient carbon capture from wet flue gas, a solid adsorbent for separating CO2 from wet flue gas, and a breakthrough experiment designed to detect the actual adsorption and separation of the sample. The method is: at room temperature of 25°C, 4g10X@PVDF (35,600) is loaded into a quartz column with an inner diameter of 8mm, and one end of the quartz column is connected to a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) with a flow rate of 2ml / min (i.e., a space velocity of 2.88h -1 ), and the other end is connected to a mass spectrometer to detect the adsorption and separation of the gas. The sample column can be heated at 150℃ for 2h in a helium atmosphere to desorb and regenerate the sample CO2.

[0064] The experimental graph of 10X@PVDF (35,600) for 4 consecutive gas adsorption and desorption cycles of mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that in Example 1.

[0065] Embodiment 5:

[0066] A hydrophobically modified zeolite molecular sieve and a preparation method and application thereof, the steps are as follows:

[0067] (1) Weigh 20g of 13X molecular sieve and activate it at 450℃ for 2h, then immerse it in 7g of polyvinylidene fluoride (PVDF) and 20g of acetone to form a mixed solution, stir overnight, and then place the mixture in a forced air drying oven at 80℃ to dry for 6h.

[0068] (2) The mixture was placed in a tubular furnace, heated to 500° C. at a heating rate of 5° C. / min in a nitrogen atmosphere, and kept at this temperature for 5 h to obtain a fluorinated carbon-coated zeolite molecular sieve 13X@PVDF (35,500).

[0069] The cross-sectional carbon element line scanning image, XRD spectrum and CO2 adsorption isotherm at 273K of the obtained 13X@PVDF (35,500) are similar to those in Example 1.

[0070] An application of a fluorinated carbon-coated zeolite molecular sieve for efficient carbon capture from wet flue gas, a solid adsorbent for separating CO2 from wet flue gas, and a breakthrough experiment designed to detect the actual adsorption and separation of the sample. The method is: at room temperature of 25°C, 4g13X@PVDF (35,500) is loaded into a quartz column with an inner diameter of 8mm, and one end of the quartz column is connected to a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) with a flow rate of 2ml / min (i.e., a space velocity of 2.88h -1 ), and the other end is connected to a mass spectrometer to detect the adsorption and separation of the gas. The sample column can be heated at 150℃ for 2h in a helium atmosphere to desorb and regenerate the sample CO2.

[0071] The experimental graph of 13X@PVDF (35,500) for 4 consecutive gas adsorption and desorption cycles of mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that in Example 1.

[0072] Embodiment 6:

[0073] A hydrophobically modified zeolite molecular sieve and a preparation method and application thereof, the steps are as follows:

[0074] (1) Weigh 30g of 5A molecular sieve and activate it at 550℃ for 2h, then immerse it in 7.5g of polyvinylidene fluoride (PVDF) and 25g of acetone to form a mixed solution, stir overnight, and then place the mixture in a forced air drying oven at 80℃ to dry for 6h.

[0075] (2) The mixture was placed in a tubular furnace, heated to 600° C. at a heating rate of 5° C. / min in a nitrogen atmosphere, and kept at this temperature for 5 h to obtain a fluorinated carbon-coated zeolite molecular sieve 5A@PVDF (25,600).

[0076] The cross-sectional carbon element line scanning image, XRD spectrum and CO2 adsorption isotherm at 273K of the obtained 5A@PVDF (25,600) are similar to those in Example 1.

[0077] An application of a fluorinated carbon-coated zeolite molecular sieve for efficient carbon capture from wet flue gas, a solid adsorbent for separating CO2 from wet flue gas, and a breakthrough experiment designed to detect the actual adsorption and separation of the sample. The method is: at room temperature of 25°C, 4g5A@PVDF (25,600) is loaded into a quartz column with an inner diameter of 8mm, and one end of the quartz column is connected to a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) with a flow rate of 2ml / min (i.e., a space velocity of 2.88h -1 ), and the other end is connected to a mass spectrometer to detect the adsorption and separation of the gas. The sample column can be heated at 150℃ for 2h in a helium atmosphere to desorb and regenerate the sample CO2.

[0078] The experimental diagram of 5A@PVDF (25,600) for 4 consecutive gas adsorption and desorption cycles of mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that of Example 1.

[0079] Comparative Example 1:

[0080] This comparative example uses the same raw materials and gas adsorption separation detection method as Examples 1 and 5, except that the raw material 13X is directly tested after high-temperature activation without any modification. The material quickly reaches CO2 adsorption saturation, and water vapor is preferentially adsorbed into the pores of 13X, resulting in a significant decrease in the material's CO2 adsorption.

[0081] Figure 5 This is a 13X gas adsorption separation experimental diagram for a mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v). Figure 4 By comparison, it can be seen that the coating with carbon fluoride effectively improves the material's ability to capture and separate CO2 from wet flue gas.

[0082] Comparative Example 2:

[0083] This comparative example adopts the same raw materials and gas adsorption separation detection method as Example 2, except that the raw material 4A is directly detected after high-temperature activation without any modification.

[0084] The obtained gas adsorption separation experimental diagram of 4A for mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that of Example 1. The material quickly reaches the saturation of CO2 adsorption, and water vapor is preferentially adsorbed into the pores of 4A, resulting in a significant decrease in the material's CO2 adsorption capacity.

[0085] Comparative Example 3:

[0086] This comparative example adopts the same raw material and gas adsorption separation detection method as Example 3, except that the raw material ZSM-5 is directly detected after high-temperature activation without any modification.

[0087] The gas adsorption separation experimental diagram of the obtained ZSM-5 for the mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that in Example 1. The material quickly reaches the saturation of CO2 adsorption, and water vapor is preferentially adsorbed into the pores of ZSM-5, resulting in a significant decrease in the material's CO2 adsorption capacity.

[0088] Comparative Example 4:

[0089] This comparative example uses the same raw materials and gas adsorption separation detection method as Example 4, except that the raw materials are directly tested after 10X high-temperature activation without any modification.

[0090] The obtained 10X gas adsorption separation experimental diagram for mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that in Example 1. The material quickly reaches the saturation of CO2 adsorption, and water vapor is preferentially adsorbed into the pores of 10X, resulting in a significant decrease in the material's CO2 adsorption capacity.

[0091] Comparative Example 5:

[0092] This comparative example adopts the same raw materials and gas adsorption separation detection method as Example 6, except that the raw material 5A is directly detected after high-temperature activation without any modification.

[0093] The obtained gas adsorption separation experimental diagram of 5A for mixed gas (H2O / CO2 / N2, 10:14:76, v:v:v) is similar to that of Example 1. The material quickly reaches the saturation of CO2 adsorption, and water vapor is preferentially adsorbed into the pores of 5A, resulting in a significant decrease in the material's CO2 adsorption capacity.

[0094] In summary, the carbon fluoride-coated zeolite molecular sieve composite material in the embodiment, compared with the simple zeolite molecular sieve in the comparative example, the carbon fluoride coating blocks the adsorption of water by the zeolite molecular sieve, thereby greatly improving the CO2 capture and separation performance in wet flue gas.

[0095] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

[0096] Matters not covered by the present invention are known technologies.

Claims

1. A hydrophobically modified zeolite molecular sieve characterized by The molecular sieve comprises a zeolite molecular sieve and a carbon fluoride layer coated thereon; the thickness of the carbon fluoride layer is 2 to 6 microns; the mass of the carbon fluoride is 5% to 60% of the mass of the zeolite molecular sieve; The particle size range of the zeolite molecular sieve is 2-5 mm; The zeolite molecular sieve is specifically an X-type molecular sieve, a Y-type molecular sieve, an MFI-type molecular sieve, an A-type molecular sieve or a B-type molecular sieve; The method for preparing the hydrophobically modified zeolite molecular sieve comprises the following steps: (1). Keep the zeolite molecular sieve at 200-600°C for 1-4 hours to obtain an activated molecular sieve; (2) Immerse the activated molecular sieve in the mixed solution and stir at 20°C to 30°C for 8 to 12 hours to obtain a zeolite molecular sieve coated with a polymer containing a fluorine functional group; The mixed solution is acetone containing an organic polymer containing a fluorine functional group, the concentration of the polymer is in the range of 5wt% to 60wt%, and 10g to 30g of molecular sieve is added to every 15g to 45g of the mixed solution; (3) Place the polymer-coated zeolite molecular sieve obtained in the previous step in a 60°C to 100°C forced air drying oven and dry for 4 to 8 hours; (4) Place the dried material obtained in the previous step into a heating furnace, and under nitrogen protection, raise the temperature to 400-700°C and keep the temperature constant for 3-6 hours; (5) Cooling to room temperature and discharging the material to obtain a hydrophobically modified zeolite molecular sieve; The organic polymer containing fluorine functional groups is fluoroplastic, fluororubber and fluoro coating, specifically polytetrafluoroethylene (PTFE), soluble polytetrafluoroethylene (PFA), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE) and FKM (fluororubber).

2. The hydrophobically modified zeolite molecular sieve according to claim 1, characterized in that In the step (4), the heating rate is 5-15°C / min.

3. The use of the hydrophobically modified zeolite molecular sieve prepared as claimed in claim 1, characterized in that it is used for capturing CO2 in wet flue gas, air separation or natural gas purification.

4. The use as claimed in claim 3, characterized in that the capture of CO2 from the wet flue gas specifically comprises the following steps: passing the flue gas into a columnar reactor filled with a hydrophobically modified zeolite molecular sieve composite material to complete the capture and separation of CO2 from the wet flue gas; in, The components in the flue gas include 12~14 vol% CO2, 8~10 vol% H2O and 72~77 vol% N2; the temperature is 5~30℃, and the air velocity is 1~10h -1 .

5. The regeneration method of the hydrophobically modified zeolite molecular sieve composite material according to claim 1, comprising the following steps: In an inert gas atmosphere, keep the temperature at 120-180°C for 1-3 hours, and then cool to room temperature; The inert gas is helium.

Citation Information

Patent Citations

  • A method for hydrophobic modification of zeolite molecular sieves

    CN102992341B

  • Hydrophobically modified ZSM-5 molecular sieve and preparation method and application thereof

    CN112390270A

  • Hydrophobic modified molecular sieve as well as preparation method and application thereof

    CN114570328A

  • Hydrophobic modification method of ZSM-5 and NaY molecular sieves

    CN115228431A

  • Hydrophobic modified molecular sieve as well as preparation method and application thereof

    CN115445582A