Preparation method and application of modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst
By combining the modified carbon nitride support and Fe(NO3)3·9H2O, a high-load catalyst is formed, which solves the problems of low CO conversion rate and high selectivity of C1 by-products in the existing catalysts, and achieves high efficiency Low-carbon olefins have improved selectivity and stability.
Patent Information
- Application Number
- CN202310251028.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-15
AI Technical Summary
The existing carbon nitride-supported iron catalysts have a high CO conversion rate in Fischer-Tropsch synthesis, but the C1 by-product selectivity is high, the low-carbon olefins are low, and the product distribution is not ideal.
The modified carbon nitride support was prepared by calcining urea in deionized water, and ultrasonic stirring with Fe(NO3)3·9H2O in ethanol to form a high-load catalyst of active component Fe and support g-C3N4, through two Step surface modification improves the activity and dispersion of the catalyst.
It improves CO conversion, reduces the selectivity of C1 by-products, improves the selectivity of low-carbon olefins, and enhances the stability of the catalyst and product distribution control ability.
Smart Images

Figure CN116237075B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of Fischer-Tropsch synthesis catalysts, and in particular to a preparation method and application of a modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst. Background Art
[0002] In the early 1920s, Fischer–Tropsch synthesis (FTS) was used to form a mixture of hydrocarbons by reacting CO with H2 over heterogeneous Fe / ZnO and Co / Cr2O3 catalysts. This was the initial application of Fischer–Tropsch synthesis in industry. In this catalyst system, synthesis gas (H2 / CO) was converted into low-carbon hydrocarbons or high-carbon liquid hydrocarbons. Later, by adjusting process conditions and designing new catalysts, high-value-added low-carbon olefins and liquid fuels such as diesel and aviation kerosene could be prepared. In recent years, the one-step preparation of low-carbon olefins (C2 = -C4 = ), linear α-olefins (LAOs) and oxygenated compounds have become one of the important research areas of C1 chemistry. Low-carbon olefins and linear α-olefins are the main primary products of Fischer-Tropsch and important basic chemical raw materials. They are widely used, but they are affected by the Anderson-Schulz-Flory (ASF) product distribution. It is necessary to further regulate the product distribution, reduce the generation of by-products such as CH4 and CO2, and improve olefin selectivity. Therefore, the development of efficient catalysts is the key.
[0003] The regulation of product distribution in Fischer-Tropsch synthesis is a technical difficulty. The Fischer-Tropsch synthesis reaction mainly produces hydrocarbon substances such as alkanes and alkenes, as well as a small amount of by-products such as low-carbon alcohols and aldehydes. The reaction process is highly exothermic, leading to side reactions such as methanation and carbon deposition. The generation of H2O during the reaction promotes the water gas shift (WGS), resulting in a large amount of CO2 generation. At the same time, affected by the ASF distribution, the product composition is complex. Effective regulation of product distribution can be achieved through new catalyst design and process parameter adjustment. Supported catalysts can effectively reduce the impact of thermal effects, side reactions, etc. on product distribution to a certain extent, and have a good modulation effect on product selectivity. The choice of carrier is the key, especially some carbon-based carriers, which have rich surface groups and are easy to modify, and play an important role in regulating product distribution.
[0004] Carbon nitride (g-C3N4) is a new type of polymer semiconductor material with a two-dimensional structure. It is widely used in photocatalysis due to its excellent properties. Its raw materials are cheap, the preparation method is simple, and it has a large specific surface area, making it an ideal carrier material. There are experiments at home and abroad that use cellulose to modify Fe3O4 on the surface to improve the hydrophilicity of Fe3O4 and increase the selectivity of linear α-olefins from 5.00% to 61.50%; some researchers also use P to modify the Al2O3 carrier. After impregnation with Co, the catalyst Co / P-Al2O3 shows high activity and stability, and the CO conversion rate is increased from 22.50% to 40.60%, and C5 + The hydrocarbon selectivity increased from 73.70% to 80.20%. By modifying the surface of the material, the researchers greatly enriched the groups on the surface of the material, improved the performance of the catalyst, and effectively and purposefully regulated the distribution of the products. Although the g-C3N4-loaded iron-based catalyst has a CO conversion rate of 71.00%, its C1 byproduct (CH4, CO2) selectivity is higher and the olefin selectivity is lower.
[0005] Generally speaking, loading Fe on the surface of g-C3N4 can form a FT synthesis active phase g-C3N4 complex, but due to its strong interaction with metals, the Fischer-Tropsch reaction evaluation after loading Fe has high activity, but the selectivity of CH4 and CO2 is high, the selectivity of light olefins is low, and the product distribution is not ideal. Therefore, it is necessary to design a new preparation method of modified carbon nitride loaded iron Fischer-Tropsch synthesis catalyst to solve the above technical problems. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst and its application, which effectively improves the dispersion of the iron component on the catalyst surface, thereby improving the conversion rate of CO, and at the same time reduces the selectivity of C1 by-products and improves the selectivity of light olefins.
[0007] The present invention is achieved in that:
[0008] The present invention provides a method for preparing a modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst, comprising the following steps:
[0009] (1) dissolving a certain amount of urea in deionized water, mixing thoroughly to obtain a mixture A, and placing the mixture A in a muffle furnace and calcining at high temperature to obtain g-C3N4;
[0010] (2) taking a certain amount of g-C3N4 obtained in step (1) and adding it to hydrogen peroxide, stirring it thoroughly, centrifuging and drying it to obtain hydrogen peroxide-modified g-C3N4, which is denoted as B;
[0011] (3) adding B and urea to deionized water in a certain mass ratio, placing the mixture in a reactor for high temperature treatment, centrifuging and drying the mixture after the treatment to obtain a modified carbon nitride support, which is recorded as C;
[0012] (4) adding C and Fe(NO3)3·9H2O in a certain mass ratio into ethanol, stirring after ultrasonication to obtain a mixture, and further drying and calcining to obtain a catalyst;
[0013] The mass ratio of the active component Fe to the carrier g-C3N4 in the obtained catalyst is 0.25-0.5.
[0014] Furthermore, in step (1), urea is 5-20 g, deionized water is 2-30 mL, the calcination temperature is 400-500° C., and the calcination time is 1-3 h.
[0015] Furthermore, in step (2), the mass of g-C3N4 is 2-4 g, and the mass of hydrogen peroxide is 100-200 mL.
[0016] Furthermore, in step (2), deionized water is used for centrifugation 4 to 5 times, the drying temperature is 60 to 80° C., and the drying time is 12 to 16 hours.
[0017] Furthermore, in step (3), the mass ratio of urea to B is 4 to 9, the amount of deionized water is 200 to 400 mL, and the mass of B is 1 to 4 g.
[0018] Furthermore, in step (3), the reactor is a polytetrafluoroethylene reactor, the temperature in the reactor is 150-200° C., and the reaction time is 2-6 hours.
[0019] Furthermore, in step (4), the mass ratio of Fe(NO3)3·9H2O to C is 1.81-3.61, the mass of C is 1-3 g, and 50-150 mL of ethanol.
[0020] Furthermore, in step (4), the ultrasonic time is 10-20 min, and the stirring time is 12-16 h.
[0021] Furthermore, in step (4), the drying temperature is 80-90° C., the drying time is 2-4 h, the calcination temperature is 300-500° C., and the insulation time is 3-6 h.
[0022] The present invention also provides the use of the modified carbon nitride supported iron Fischer-Tropsch synthesis catalyst prepared by the above preparation method in Fischer-Tropsch synthesis, which can improve the CO conversion rate, reduce the selectivity of C1 by-products (CH4, CO2) in product distribution, and improve the selectivity of light olefins (C2 = -C4 = )’s selectivity.
[0023] The present invention has the following beneficial effects:
[0024] 1. The supported catalyst directly calcined by adding water to urea in the present invention has a large specific surface area, which is conducive to the dispersion of active components, has a high loading amount of active components, and improves the FTS catalytic activity;
[0025] 2. The present invention can effectively regulate product distribution through two-step surface modification;
[0026] 3. The catalyst of the present invention is used for Fischer-Tropsch reaction under mild reaction conditions. When reacting at 280°C, the CO conversion rate can reach 68.03% to 76.62%, the CH4 selectivity and CO2 selectivity are both at low values, the selectivity of light olefins can reach 43.67%, the O / P value is 4.2, the stability is good, the CO conversion rate is improved, and the selectivity of light olefins is improved while the selectivity of C1 by-products is reduced;
[0027] 4. The raw materials and reagents used in the catalyst of the present invention are all non-precious metals, green and environmentally friendly, cheap and easy to obtain, the preparation method is simple, the process is easy to operate and repeat, the time consumption is short, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a scanning electron microscope image of the modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst prepared in the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present invention provides a method for preparing a modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst, comprising the following steps:
[0032] (1) dissolving a certain amount of urea in deionized water, mixing thoroughly to obtain a mixture A, and placing the mixture A in a muffle furnace and calcining at high temperature to obtain g-C3N4;
[0033] (2) adding a certain amount of g-C3N4 into hydrogen peroxide, stirring thoroughly, centrifuging and drying to obtain hydrogen peroxide-modified g-C3N4, denoted as B;
[0034] (3) adding B and urea to deionized water in a certain mass ratio, placing the mixture in a reactor for high temperature treatment, centrifuging and drying the mixture after the treatment to obtain a modified carbon nitride support, which is recorded as C;
[0035] (4) adding C and Fe(NO3)3·9H2O in a certain mass ratio into ethanol, stirring after ultrasonication to obtain a mixture, and further drying and calcining to obtain a catalyst;
[0036] The mass ratio of the active component Fe to the carrier g-C3N4 in the obtained catalyst is 0.25-0.5.
[0037] The g-C3N4 obtained by calcining the mixture A obtained by adding urea to deionized water in step (1) of the preparation method of the present invention has a large specific surface area. The modification process of steps (2) and (3) can prepare a modified carrier with richer surface groups. The average pore size of the modified carrier becomes larger, and the average pore size of C can reach 42.28nm, which is convenient for the loading and dispersion of Fe, forming a large number of defects, which will increase the adsorption of CO by the catalyst, thereby improving the conversion rate of CO. The average pore size of the carrier B obtained by only hydrogen peroxide modification is smaller than that of C, which is not conducive to the diffusion of substances, increases the probability of secondary reactions, and makes the olefin selectivity low. Continuing to modify by adding urea, its surface groups and electronic structure are changed, and the hydrophilicity is enhanced. The large-pore carrier C obtained is conducive to the loading and dispersion of Fe. The carrier loaded with iron can weaken the secondary reaction of Fischer-Tropsch synthesis, reduce the selectivity of by-products, improve the selectivity of olefins and reduce the selectivity of C1 by-products.
[0038] After calcination in step (4), a high-load catalyst is obtained by an impregnation method, which contains two different iron phases, an iron phase with strong interaction between Fe and the carrier and an iron phase with weak interaction. The iron phase with strong interaction is more difficult to reduce. If the loading is low, its content will be higher, making it difficult to reduce the iron phase, and the CO conversion rate will be lower. Therefore, the high-load catalyst of the present invention can ensure a higher CO conversion rate.
[0039] like Figure 1As shown, the catalyst Fe prepared by the present invention has good dispersibility and a larger pore size, wherein the loading amount of the active ingredient Fe is higher, and the mass ratio of Fe to the carrier g-C3N4 can reach 0.25 to 0.5, thereby ensuring a higher CO conversion rate. At the same time, the prepared g-C3N4 has a larger specific surface area, and is more convenient for Fe loading after the modification process of steps (2) and (3), forming a large number of defects. The large pore size is conducive to the dispersion of Fe loading, and the obtained iron-loaded carrier can weaken the secondary reaction of Fischer-Tropsch synthesis, reduce the selectivity of by-products, improve the selectivity of olefins and reduce the selectivity of C1 by-products.
[0040] The following specific examples are used to illustrate this in detail. In all the following examples, the mass ratio of Fe to carrier carbon nitride is calculated by an inductively coupled plasma emission spectrometer (ICP).
[0041] Example 1
[0042] The preparation method of the Fe-based Fischer-Tropsch synthesis catalyst of the present invention comprises the following steps:
[0043] (1) Add 5 g of urea to 2 mL of distilled water to obtain A; place A in a muffle furnace and calcine, increase the temperature to 400 °C, and maintain this temperature for 1 hour to obtain g-C3N4.
[0044] (2) 2 g of g-C3N4 was added to 100 mL of hydrogen peroxide and stirred at room temperature for 1 h. The deionized water was centrifuged four times and dried at 60 °C to obtain a H2O2-modified support, which was denoted as B.
[0045] (3) Take 2 g of B and 8 g of urea and add them to 200 ml of deionized water. Transfer the mixture to a polytetrafluoroethylene reactor and raise the temperature to 130°C for 2 h. The NH3·H2O-modified support is obtained and is marked as C.
[0046] (4) 4.0400 g of Fe(NO3)3·9H2O was weighed and dissolved in 50 mL of ethanol, followed by the addition of 2 g of C, and the mixture was ultrasonically treated for 10 min. Thereafter, the resulting mixture was stirred for 12 h. The solvent was removed, and the resulting solid was dried at 80°C for 1 h and then calcined at 300°C for 3 h. The obtained catalyst was denoted as 1-Fe / g-C3N4.
[0047] In the catalyst prepared in this example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.28.
[0048] Example 2
[0049] The preparation method of the Fe-based Fischer-Tropsch synthesis catalyst of the present invention comprises the following steps:
[0050] (1) Add 7 g of urea to 5 mL of distilled water to obtain A. Place A in a muffle furnace and calcine, raise the temperature to 450 °C, and maintain this temperature for 2 h to obtain g-C3N4.
[0051] (2) 3 g of g-C3N4 was added to 150 mL of hydrogen peroxide and stirred at room temperature for 2 h. The deionized water was centrifuged 5 times and dried at 60 °C to obtain a H2O2-modified support, which was denoted as B.
[0052] (3) 1 g of B and 9 g of urea were added to 300 ml of deionized water, and the resulting mixture was transferred to a polytetrafluoroethylene reactor, and the temperature was raised to 150°C and maintained for 4 h. The NH3·H2O-modified support was obtained, which was recorded as C.
[0053] (4) 5.43 g of Fe(NO3)3·9H2O was weighed and dissolved in 75 mL of ethanol, followed by the addition of 3 g of C, and the mixture was then ultrasonicated for 15 min. Thereafter, the resulting mixture was stirred for 14 h. The solvent was removed, and the resulting solid was dried at 85°C for 2 h and then calcined at 400°C for 4 h. The obtained catalyst was denoted as 2-Fe / g-C3N4.
[0054] In the catalyst prepared in this example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.25.
[0055] Example 3
[0056] The preparation method of the Fe-based Fischer-Tropsch synthesis catalyst of the present invention comprises the following steps:
[0057] (1) Add 10 g of urea to 10 mL of distilled water to obtain A. Place A in a muffle furnace and calcine, raise the temperature to 400 °C, and maintain this temperature for 2 h to obtain g-C3N4.
[0058] (2) 4 g of g-C3N4 was added to 200 mL of hydrogen peroxide and stirred at room temperature for 4 h. The deionized water was centrifuged 5 times and dried at 70 °C to obtain a H2O2-modified support, which was denoted as B.
[0059] (3) 2 g of B and 10 g of urea were added to 400 ml of deionized water, and the resulting mixture was transferred to a polytetrafluoroethylene reactor, and the temperature was raised to 140°C and maintained for 2 h. The NH3·H2O-modified support was obtained, which was recorded as C.
[0060] (4) 10.83 g of Fe(NO3)3·9H2O was weighed and dissolved in 100 mL of ethanol, and then 3 g of C was added, and the mixture was ultrasonically treated for 20 min. Thereafter, the resulting mixture was stirred for 16 h. The solvent was removed, and the resulting solid was dried at 90°C for 2 h and then calcined at 450°C for 3 h. The obtained catalyst was denoted as 3-Fe / g-C3N4.
[0061] In the catalyst prepared in this example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.5.
[0062] Example 4
[0063] The preparation method of the Fe-based Fischer-Tropsch synthesis catalyst of the present invention comprises the following steps:
[0064] (1) Add 15 g of urea to 15 mL of distilled water to obtain A. Place A in a muffle furnace and calcine, raise the temperature to 450 °C, and maintain this temperature for 3 h to obtain g-C3N4.
[0065] (2) 3 g of g-C3N4 was added to 170 mL of hydrogen peroxide and stirred at room temperature for 3 h. The deionized water was centrifuged 5 times and dried at 80 °C to obtain a H2O2-modified support, which was denoted as B.
[0066] (3) 4 g of B and 36 g of urea were added to 400 ml of deionized water, and the resulting mixture was transferred to a polytetrafluoroethylene reactor, and the temperature was raised to 200° C. and maintained for 2 h. The NH 3 · H 2 O-modified support was obtained, which was recorded as C.
[0067] (4) 2.53 g of Fe(NO3)3·9H2O was weighed and dissolved in 50 mL of ethanol, followed by the addition of 1 g of C, and the mixture was then ultrasonicated for 15 min. Thereafter, the resulting mixture was stirred for 12 h. The solvent was removed, and the resulting solid was dried at 80°C for 1 h and then calcined at 500°C for 6 h. The obtained catalyst was denoted as 4-Fe / g-C3N4.
[0068] In the catalyst prepared in this example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.35.
[0069] Example 5
[0070] The preparation method of the Fe-based Fischer-Tropsch synthesis catalyst of the present invention comprises the following steps:
[0071] (1) Add 20 g of urea to 30 mL of distilled water to obtain A. Place A in a muffle furnace and calcine, raise the temperature to 500 °C, and maintain this temperature for 3 h to obtain g-C3N4.
[0072] (2) 4 g of g-C3N4 was added to 200 mL of hydrogen peroxide, stirred at room temperature for 4 h, centrifuged 5 times with deionized water, and dried at 80 °C to obtain a H2O2-modified support, denoted as B.
[0073] (3) 3 g of B and 21 g of urea were added to 350 ml of deionized water, and the resulting mixture was transferred to a polytetrafluoroethylene reactor, and the temperature was raised to 135° C. and maintained for 6 h. The NH 3 · H 2 O-modified support was obtained, which was recorded as C.
[0074] (4) 6.06 g of Fe(NO3)3·9H2O was weighed and dissolved in 150 mL of ethanol, followed by the addition of 3 g of C, and the mixture was then ultrasonicated for 20 min. Thereafter, the resulting mixture was stirred for 16 h. The solvent was removed, and the resulting solid was dried at 90°C for 4 h and then calcined at 500°C for 6 h. The obtained catalyst was denoted as 5-Fe / g-C3N4.
[0075] In the catalyst prepared in this example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.28.
[0076] Example 6
[0077] The preparation method of the Fe-based Fischer-Tropsch synthesis catalyst of the present invention comprises the following steps:
[0078] (1) Add 10 g of urea to 15 mL of distilled water to obtain A. Place A in a muffle furnace and calcine, raise the temperature to 450 °C, and maintain this temperature for 1 h to obtain g-C3N4.
[0079] (2) 4 g of g-C3N4 was added to 100 mL of hydrogen peroxide, stirred at room temperature for 2 h, centrifuged 5 times with deionized water, and dried at 70 °C to obtain a H2O2-modified support, denoted as B.
[0080] (3) 4 g of B and 20 g of urea were added to 370 ml of deionized water, and the resulting mixture was transferred to a polytetrafluoroethylene reactor, and the temperature was raised to 145°C and maintained for 2 h. The NH3·H2O-modified support was obtained, which was recorded as C.
[0081] (4) 8.68 g of Fe(NO3)3·9H2O was weighed and dissolved in 50 mL of ethanol, followed by the addition of 3 g of C, and the mixture was then ultrasonicated for 10 min. Thereafter, the resulting mixture was stirred for 15 h. The solvent was removed, and the resulting solid was dried at 90°C for 1 h and then calcined at 450°C for 3 h. The obtained catalyst was denoted as 6-Fe / g-C3N4.
[0082] In the catalyst prepared in this example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.4.
[0083] Example 7
[0084] The preparation method of the Fe-based Fischer-Tropsch synthesis catalyst of the present invention comprises the following steps:
[0085] (1) Add 15 g of urea to 25 mL of distilled water to obtain A. Place A in a muffle furnace and calcine, raise the temperature to 500 °C, and maintain this temperature for 1 h to obtain g-C3N4.
[0086] (2) 2 g of g-C3N4 was added to 150 mL of hydrogen peroxide and stirred at room temperature for 3 h. The deionized water was centrifuged 5 times and dried at 75 °C to obtain a H2O2-modified support, which was denoted as B.
[0087] (3) 3.5 g of B and 14 g of urea were added to 380 ml of deionized water, and the resulting mixture was transferred to a polytetrafluoroethylene reactor, and the temperature was raised to 145° C. and maintained for 5 h. The NH 3 · H 2 O-modified support was obtained, which was recorded as C.
[0088] (4) 9.76 g of Fe(NO3)3·9H2O was weighed and dissolved in 50 mL of ethanol, followed by the addition of 3 g of C, and the mixture was then ultrasonicated for 15 min. Thereafter, the resulting mixture was stirred for 16 h. The solvent was removed, and the resulting solid was dried at 80°C for 4 h and then calcined at 450°C for 3 h. The obtained catalyst was designated as 7-Fe / g-C3N4.
[0089] In the catalyst prepared in this example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.45.
[0090] Comparative Example 1
[0091] A method for preparing an Fe-based Fischer-Tropsch synthesis catalyst, the method comprising the following steps:
[0092] (1) 15 g of melamine was placed in a muffle furnace and calcined. After cooling, the mixture was ground to obtain g-C3N4.
[0093] (2) 1.44 g of Fe(NO3)3·9H2O was weighed and dissolved in 100 mL of ethanol, followed by the addition of 2 g of g-C3N4, and the mixture was then ultrasonicated for 15 min. Thereafter, the resulting mixture was stirred for 16 h. The solvent was removed, and the resulting solid was dried at 80°C for 4 h and then calcined at 450°C for 3 h. The obtained catalyst was denoted as a-Fe / g-C3N4.
[0094] In the catalyst prepared in this comparative example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.10.
[0095] Comparative Example 2
[0096] A method for preparing an Fe-based Fischer-Tropsch synthesis catalyst, the method comprising the following steps:
[0097] (1) 20 g of melamine was placed in a muffle furnace and calcined. After cooling, the mixture was ground to obtain g-C3N4.
[0098] (2) 2.59 g of Fe(NO3)3·9H2O was weighed and dissolved in 150 mL of ethanol, and then 3 g of g-C3N4 was added, and the mixture was ultrasonically treated for 16 min. Thereafter, the resulting mixture was stirred for 12 h. The solvent was removed, and the resulting solid was dried at 90°C for 4 h and then calcined at 450°C for 6 h. The obtained catalyst was denoted as b-Fe / g-C3N4.
[0099] In the catalyst prepared in this comparative example, the mass ratio of the active component Fe to the carrier carbon nitride is 0.12.
[0100] The catalysts prepared in Examples 1 to 7 and Comparative Examples 1 to 2 were used in a 66.6% H2, 33.3% CO atmosphere. A fixed bed reactor was used under the following operating conditions: 280°C, 2 MPa, 2000 h -1 The catalytic performance is shown in Table 1.
[0101] Table 1 Performance test results of catalysts prepared in Examples 1 to 7 and Comparative Examples 1 to 2
[0102]
[0103] As can be seen from Table 1, compared with Comparative Example 1 and Comparative Example 2, the catalyst prepared in the embodiment of the present invention has a higher Fe loading. The supported catalyst directly calcined by adding water to urea has a larger specific surface area, which is conducive to the dispersion of active components. Through two-step surface modification, the product distribution is effectively regulated. When applied to Fischer-Tropsch synthesis, it has a higher CO conversion rate, while reducing the selectivity of C1 by-products (CO2, CH4) and improving the selectivity of light olefins (C2-C4 = ) selectivity, and the final catalyst has a high loading of active components and good FTS catalytic activity.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst, characterized in that: The following steps are involved: (1) dissolving a certain amount of urea in deionized water, mixing thoroughly to obtain a mixture A, and placing the mixture A in a muffle furnace and calcining at high temperature to obtain g-C3N4; Wherein, urea 5-20g, deionized water 2-30mL, calcination temperature is 400-500℃, calcination time is 1-3h; (2) taking a certain amount of g-C3N4 obtained in step (1) and adding it to hydrogen peroxide, stirring it thoroughly, centrifuging and drying it to obtain g-C3N4 modified with hydrogen peroxide, which is denoted as B; wherein the mass of g-C3N4 is 2-4 g, and the hydrogen peroxide is 100-200 mL; (3) adding B and urea to deionized water in a certain mass ratio, placing the mixture in a reactor for high temperature treatment, centrifuging and drying the mixture after the treatment to obtain a modified carbon nitride support, denoted as C; wherein the mass ratio of urea to B is 4 to 9, the deionized water is 200 to 400 mL, and the mass of B is 1 to 4 g; (4) adding C and Fe(NO3)3·9H2O in a certain mass ratio to ethanol, stirring to obtain a mixture after ultrasonication, and continuing to dry and calcine to obtain a catalyst; wherein the mass ratio of Fe(NO3)3·9H2O to C is 1.81-3.61, the mass of C is 1-3 g, and 50-150 mL of ethanol; The mass ratio of the active component Fe to the carrier g-C3N4 in the obtained catalyst is 0.25-0.
5.
2. The method for preparing the modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst according to claim 1, characterized in that: In step (2), centrifuge with deionized water for 4 to 5 times, dry at 60 to 80° C., and dry for 12 to 16 hours.
3. The method for preparing the modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst according to claim 1, characterized in that: In step (3), the reactor is a polytetrafluoroethylene reactor, the temperature in the reactor is 150-200° C., and the reaction time is 2-6 hours.
4. The method for preparing the modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst according to claim 1, characterized in that: In step (4), the ultrasonic time is 10-20 min and the stirring time is 12-16 h.
5. The method for preparing the modified carbon nitride-supported iron Fischer-Tropsch synthesis catalyst according to claim 1, characterized in that: In step (4), the drying temperature is 80-90° C., the drying time is 2-4 hours, the calcination temperature is 300-500° C., and the insulation time is 3-6 hours.
6. Use of the modified carbon nitride supported iron Fischer-Tropsch synthesis catalyst prepared by any one of the methods of claims 1 to 5 in Fischer-Tropsch synthesis.