A method for purifying and using wet phosphoric acid desulfurization bottom slag
Through conditioning and classification treatment, the problem of difficult solid-liquid separation during the purification process of wet phosphoric acid desulfurization bottom residue was solved, the production of heavy calcium and ordinary calcium was realized, the phosphoric acid recovery rate and resource utilization rate were improved, and the desulfurization bottom residue was realized. Full resource treatment of slag.
Patent Information
- Application Number
- CN202310278900.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-21
AI Technical Summary
During the purification process, the wet phosphoric acid desulfurization bottom residue has problems such as low P2O5 concentration, high solid content, high viscosity of liquid phosphoric acid, difficulty in filtration, and a large amount of trapped liquid phosphoric acid, resulting in low resource recovery and treatment efficiency, and the existing technology is not yet available. can effectively utilize these characteristics.
Conditioning agent and filter aid are used for conditioning treatment, and heavy calcium and ordinary calcium are obtained through filtration and washing steps. The clear liquid is reacted with phosphate rock powder to produce heavy calcium, and the filter cake is mixed with calcium carbonate or lime. Powder reaction is used to prepare calcium chloride to achieve full utilization of resources.
Through hierarchical treatment and reaction, the P2O5 recovery rate and resource utilization rate of desulfurization bottom residue are improved, full resource utilization without the production of toxic and harmful substances is achieved, solid waste discharge is reduced, and phosphoric acid recovery efficiency is improved.
Smart Images

Figure CN116239139B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource recovery and processing production, and in particular to a method for purifying and using wet-process phosphoric acid desulfurization bottom slag. Background Art
[0002] After the concentrated wet phosphoric acid, only after desulfurization can it enter the deep purification operation and finally obtain qualified purified phosphoric acid. Therefore, desulfurization wet phosphoric acid purification is an indispensable operation unit. In the desulfurization process, due to the addition of Ca 2+ , Ba 2+ + and other cations, so when forming calcium sulfate salts, barium sulfate salts, and phosphates, some other crystals such as Fe, Al, and F complex salts will also precipitate from the phosphoric acid solution, and sandwich a certain amount of liquid phosphoric acid between the crystals to form desulfurization slag, which is precipitated and separated from the phosphoric acid. Therefore, the desulfurization slag has the following characteristics: 1), low P2O5 concentration; 2), high solid content; 3), low liquid phosphoric acid concentration, high viscosity, low H+ concentration, and poor chemical activity; 4), fine crystals, difficult to filter, and a large amount of liquid phosphoric acid is sandwiched between the crystals; 5), due to the presence of phosphate, Fe, Al, and F complexes, the viscosity of the liquid phosphoric acid is high.
[0003] A large amount of desulfurization slag is produced during the purification process of wet phosphoric acid. The solid content in the desulfurization slag is 78-80%, and the phosphoric acid content is 20-22%. So far, there has been no report on the resource recovery of the desulfurization slag. Summary of the invention
[0004] The object of the present invention is to provide a method for purifying and using bottom slag of wet phosphoric acid desulfurization, which uses a conditioning agent and a filter aid to condition the material, filters the conditioned material, and then adopts the principle of graded treatment to produce heavy calcium and ordinary calcium.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for purifying and using wet phosphoric acid desulfurization bottom slag, characterized in that it comprises the following steps:
[0007] A. Tempering treatment: add the desulfurized bottom slag into the tempering tank for tempering treatment, continuously add tempering agent and filter aid during the tempering treatment, the amount of filter aid added is 1-5%, and the tempering agent is added mainly according to the pH value and slurry viscosity, the stirring speed is 80-120 rpm, the tempering time is 4 hours, and the tempered slurry is obtained;
[0008] B. filtration, conveying the conditioned slurry obtained in step A to a plate-and-frame filter press by a liquid pump for filtration to obtain a clear liquid and a filter cake;
[0009] C. Heavy calcium production, mixing the clear liquid obtained in step B with phosphate rock powder, granulating, and drying to obtain heavy calcium;
[0010] D. Filter cake washing: washing the filter cake obtained in step B, continuously adding hot water during the washing process, and controlling the temperature of the hot water at 30-45° C. to obtain a washing liquid;
[0011] E. Secondary filtration: The washing liquid in step D is transported to a plate-and-frame filter press through a liquid pump for secondary filtration to obtain a secondary filter cake and a filtrate, and the filtrate is returned to step A for use as a diluent;
[0012] F. Production of general calcium: the secondary filter cake obtained in step E is mixed with calcium carbonate or lime powder, granulated and dried to prepare general calcium.
[0013] As a further preferred embodiment of the present invention, the filter aid in step A is diatomaceous earth or attapulgite powder, or a mixture of the two.
[0014] As a further preferred embodiment of the present invention, the conditioning agent in step A is lime or other alkaline substances.
[0015] The beneficial effects of the present invention are mainly reflected in that the surface activity of the desulfurization bottom slag is changed by adding a filter aid and a conditioning agent, so that solid-liquid separation is conveniently performed, the separated clear liquid is reacted with phosphate rock powder to produce heavy calcium, the filter cake is washed and then filtered for a second time, and the obtained secondary filter cake is reacted with calcium carbonate or lime powder to produce ordinary calcium, the resource treatment is thorough, no toxic and harmful substances are produced, and basically the full resource utilization of the desulfurization bottom slag is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] From March 7 to March 16, our company sampled the desulfurization bottom slag, and the quality of the samples is as follows:
[0019]
[0020] In view of the above characteristics of desulfurized bottom slag and the demand of phosphate fertilizer market, our development and utilization plan mainly consists of two stages:
[0021] 1. The desulfurization bottom residue is separated by filter pressing to obtain liquid phosphoric acid to the maximum extent, and the P2O5 concentration in the filter cake is reasonably controlled for comprehensive utilization to achieve no solid waste discharge.
[0022] 2. The filtrate and filter cake are used in the production of GTSP, GDSP and GSSP respectively.
[0023] 1. Classification and separation of desulfurization bottom slag
[0024] Our company has conducted several separation and classification experiments on the desulfurization bottom slag of Yunnan Phosphate Group Haikou Phosphate Co., Ltd. The results are as follows
[0025] 1. Filtrate quality, yield and recovery rate
[0026]
[0027] 2. Filter cake quality, yield and recovery rate
[0028]
[0029] 3. Comprehensive yield and recovery rate of filtrate and filter cake
[0030]
[0031] From the above experimental results, it can be seen that
[0032] 1) The desulfurization bottom slag of Yunnan Phosphate Group Haikou Phosphate Co., Ltd. was sampled for ten consecutive days, with a single-day comprehensive sample taken every two days, for a total of four batches of samples; 2) The P2O5 concentration of the filtrate of the desulfurization bottom slag was between 30% and 34.5%; the solid content was between 55.42% and 78.55%; 3) Due to the high Fe3+ and Al3+ content in the desulfurization bottom slag, the viscosity of the liquid phosphoric acid was particularly large, and it was particularly difficult to filter. Although filter aids were added, the recovery rate of the clear liquid was still very low. Also because of the high Fe3+ and Al3+ content, in the subsequent clear liquid and filter cake It is difficult to obtain products with high water-soluble phosphorus by processing GTSP and GSSP; 4). The concentration of P2O5 in the filtrate is between 41.21% and 46.36%; the solid content is about 7%, and the recovery rate of the filtrate is between 23.19% and 34%; 4). The total phosphorus of the filter cake P2O5 is between 25.77% and 27.73%, the effective phosphorus is between 19.98% and 21.72%, the free acid is between 14.28% and 22.72%, the solid content is between 91.18% and 87.44%, and the recovery rate is between 62% and 74.16%. The free acid of the filter cake is very low, and it is no longer possible to further decompose the phosphate rock powder. It can only be directly synthesized into ordinary superphosphate by using calcium carbonate powder and lime powder under the condition of controlling the free acid;
[0033] 5) The total yield reflected in the experimental data is greater than 100% because a certain amount of filter aid must be added during the desulfurization bottom slag filtration separation process to maximize the recovery of liquid phase substances in the low slag and obtain a higher acid recovery rate; 6) The filter press used in the experiment is a fully hydraulic filter press, and the filter press used in large-scale production is a plate and frame filter press. The filtration pressure will be reduced, and the actual production filtrate recovery rate will be reduced.
[0034] 2. Filtrate is used to produce GTSP
[0035] In view of the concentration and other properties of the filtrate, this part of the filtrate can be used for the production of GTSP. Since Hailin and Yunnan Shanshi Chemical Co., Ltd. both have many years of experience in the production of GTSP, their production processes and methods will not be described in detail here.
[0036] 3. Filter cake is used to produce GSSP
[0037] 1) Since the P2O5 concentration and H+ concentration in the filter cake are already very low, and it contains a large amount of Fe, Al, and F complexes, it is difficult to decompose the phosphate rock powder in this part of the filter cake; calcium carbonate and lime have to be used to neutralize the free acid contained in it to obtain low-concentration superphosphate, namely ordinary calcium;
[0038] 2) The filter cake is mixed and chemically processed with the measured calcium carbonate powder in a double-shaft mixer, and then turned over, matured and neutralized to obtain the SSP semi-finished product. The semi-finished product is then granulated, dried, screened, and other processes to obtain the GSSP finished product.
[0039] 4. For example, in the production of 1-36-5S GDSP, heavy calcium and calcium-rich semi-finished products are further neutralized with ammonia, and then a certain amount of sulfur is added, and then granulation, drying, screening and other processes are carried out. One ton of GDSP product can consume 0.78 tons of heavy calcium (equivalent to heavy calcium finished product), 0.12 tons of ordinary calcium (equivalent to ordinary calcium finished product), 0.06 tons of ammonium sulfate and 0.06 tons of sulfur.
[0040] 5. Use of Phosphoric Acid in Final Products
[0041] 1. After preliminary connection with Yunnan Phosphate Group Haikou Phosphate Co., Ltd., in order to ensure the smooth implementation of the loading, unloading and transportation of desulfurization bottom slag, it is expected that after large-scale operation, the preliminary quality of the desulfurization bottom slag will be determined to be a P2O5 concentration of 1.5; solid content of about 60%. Comparing the experimental data, it is relatively close to the data from March 14 to March 17.
[0042] 2. Considering the differences between large-scale production and experimental conditions, the P2O5 recovery rate in the filtrate phosphoric acid was 30% and the P2O5 recovery rate in the filter cake was 67.5%.
[0043] 3. In summary, each hundred tons can produce the following products:
[0044] (1) 44% GTSP 0.84 tons (1*0.3*2.8); 20% available phosphorus GSSP 3.3 tons (0.7 / 21%);
[0045] (2) GDSP of 1-36-5S: 1.08 tons; GSSP of 20% available phosphorus: 3.15 tons (0.7 / 21%-1.08*0.12).
[0046] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for purifying and using wet-process phosphoric acid desulfurization bottom slag, characterized in that: It includes the following steps: A. Tempering treatment: add the desulfurized bottom slag into the tempering tank for tempering treatment, continuously add tempering agent and filter aid during the tempering treatment, the amount of filter aid added is 1-5%, and the tempering agent is added mainly according to the pH value and slurry viscosity, the stirring speed is 80-120 rpm, the tempering time is 4 hours, and the tempered slurry is obtained; B. filtration, conveying the conditioned slurry obtained in step A to a plate-and-frame filter press by a liquid pump for filtration to obtain a clear liquid and a filter cake; C. Heavy calcium production, mixing the clear liquid obtained in step B with phosphate rock powder, granulating, and drying to obtain heavy calcium; D. Filter cake washing: washing the filter cake obtained in step B, continuously adding hot water during the washing process, and controlling the temperature of the hot water at 30-45° C. to obtain a washing liquid; E. Secondary filtration: The washing liquid in step D is transported to a plate-and-frame filter press through a liquid pump for secondary filtration to obtain a secondary filter cake and a filtrate, and the filtrate is returned to step A for use as a diluent; F. Production of general calcium, mixing the secondary filter cake obtained in step E with calcium carbonate or lime powder, granulating, and drying to prepare general calcium; The conditioning agent in step A is lime or other alkaline substances.
2. The method for purifying and using wet phosphoric acid desulfurization bottom slag according to claim 1, characterized in that: In the step A, the filter aid is diatomaceous earth or attapulgite powder, or a mixture of the two.
3. The method for purifying and using wet phosphoric acid desulfurization bottom slag according to claim 1, characterized in that: The P2O5 concentration of the filtrate of the desulfurized bottom slag is between 30% and 34.5%, and the solid content is between 55.42% and 78.55%.
Citation Information
Patent Citations
Method for preparing super phosphate by use of ardealite slag site sewage
CN103553722A
Method for preparing superphosphate
CN105330343A
Method for producing feed grade dicalcium phosphate and industrial grade phosphoric acid by phosphate ore hydrochloric acid reclamation process
CN1803589A