A 3D printing silicon carbide slurry suitable for ink direct writing technology and its preparation
By adding loofah cellulose and other additives to the silicon carbide ceramic powder, the problem of easy settlement and agglomeration of silicon carbide ceramic powder in 3D printing is solved, and stable printing and high-performance material preparation in ink direct writing technology is realized. Good electromagnetic shielding and thermal conductivity.
Patent Information
- Application Number
- CN202310092675.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-02-10
AI Technical Summary
Due to the prone to settle and agglomeration of silicon carbide ceramic powder during 3D printing, the water-based slurry is prone to material-water separation in the extrusion nozzle, which limits its application to the direct ink writing technology.
The slurry is prepared by stirring and ball milling by using a mass percentage of 40-60% silicon carbide ceramic powder and 0.3-1% loofah cellulose, combined with glycerine and carrageenan, and the slurry is processed by a specific chemical-mechanical method. Cellulose is used to improve its dispersibility.
The stable extrusion and printing of silicon carbide slurry in ink direct writing 3D printing is realized, the strength and conductivity of the structure are improved, and the electromagnetic shielding performance and controllable thermal conductivity are achieved. The printing height can exceed one centimeter. Not easy to break silk and collapse.
Smart Images

Figure CN116239385B_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a method for preparing a 3D printing silicon carbide slurry suitable for ink direct writing technology, and belongs to the technical field of 3D printing molding. Background Art
[0002] Silicon carbide ceramics are mainly covalent bonds with high bonding strength, so they have the advantages of high melting point, high hardness, high elastic modulus, good thermal conductivity and low thermal expansion coefficient. They are good high-temperature resistant structural materials and are used in various engineering fields. However, the high hardness and strength of silicon carbide make it difficult to machine and achieve lightweight preparation, which limits its development as a structural material.
[0003] 3D printing technology (additive manufacturing) is a rapid prototyping technology. This technology is based on digital model files, using powders or polymers and other bondable materials to achieve near-net shape by printing layer by layer. The development of 3D printing ceramic materials makes it possible to lightweight ceramics. Silicon carbide powder is one of the most common ceramic powders. The slurry prepared with it has the characteristics of easy sedimentation, easy agglomeration, poor fluidity, etc., and it is easy to separate the material from the water during the extrusion nozzle. Therefore, a large amount of dispersant needs to be added to the slurry.
[0004] Cellulose has the characteristics of hydrophilic cross-linking in solution and is a widely used dispersant. As a plant with a high cellulose content, loofah can be processed by chemical-mechanical method to produce nanocellulose with excellent performance. Adding it as a dispersant to ceramic slurry has the advantages of easy availability of raw materials, low cost, environmental protection and non-toxicity. Summary of the invention
[0005] The purpose of the present invention is to provide a silicon carbide slurry for 3D printing suitable for ink direct writing technology and a preparation method thereof, so as to solve the problem that silicon carbide ceramic powder is easily separated from water during the extrusion nozzle due to its own dispersion problem, thereby solving the problem that silicon carbide ceramic slurry has not been applied to the field of 3D printing with ink direct writing technology.
[0006] The technical solution of the present invention is as follows:
[0007] A 3D printing silicon carbide slurry suitable for ink direct writing technology, characterized in that: the slurry contains 40-60% silicon carbide ceramic powder and 0.3-1% loofah cellulose in mass percentage.
[0008] The slurry of the present invention may be composed of: 40-60wt.% of silicon carbide ceramic powder, 0.3-1wt.% of loofah cellulose, 10-15wt.% of glycerol, 0.05-0.1wt.% of carrageenan, and the balance of deionized water.
[0009] Wherein, the silicon carbide ceramic powder is silicon carbide whiskers and / or silicon carbide particles, with a particle size of 50nm to 50μm and a purity of 99% to 99.99%.
[0010] Wherein, the loofah cellulose is in the form of thread or sheet, and has a size range of 10 nm to 1 μm.
[0011] The present invention also provides a method for preparing the 3D printing silicon carbide slurry suitable for ink direct writing technology, which is characterized by comprising the following steps:
[0012] (1) mixing deionized water and glycerol in a volume ratio of 2:1 to 1:1 to obtain a water-oil mixture;
[0013] (2) adding loofah cellulose and carrageenan into a water-oil mixture at a material-liquid ratio of 10-50 g:1 L and 2-5 g:1 L, respectively, stirring at 80° C. for 30 min, and cooling to room temperature;
[0014] (3) Silicon carbide ceramic powder is mixed with the solution obtained in step (2) in a mass ratio of 3:1 to 2:1, and the obtained slurry is filtered through a 2000 mesh sieve.
[0015] In step (3), the mixing process of the silicon carbide ceramic powder and the solution is stirring and / or ball milling; wherein:
[0016] The stirring speed is 10-500 rpm and the stirring time is greater than 0.5 h;
[0017] The ball milling speed is 30-300 rpm, the ball milling time is 4-10 hours, and the mass ratio of the grinding balls to the slurry is greater than 0.1.
[0018] The preparation method of loofah cellulose of the present invention is:
[0019] 1) Raw material pretreatment: After washing the loofah, drying it at 80-90° C. for 4-6 h, crushing it and passing it through a 40-mesh sieve to obtain loofah powder;
[0020] 2) preparing a benzene-ethanol solution at a volume ratio of 2:1, wrapping the loofah powder with filter paper, and placing it in a Soxhlet extractor at a solid-liquid ratio of 1g:20mL to 1g:50mL, extracting at 80°C to 100°C for 6 to 12 hours; cooling naturally to room temperature, washing with deionized water for 4 to 6 times, and filtering;
[0021] 3) putting the loofah powder obtained in step 2) into a 20g / L-30g / L NaClO2 aqueous solution according to a material-liquid ratio of 1g:20mL-1g:50mL, adjusting the pH value to 2-3 with glacial acetic acid, bleaching at 80°C for 2-4h, cooling naturally to room temperature, washing with deionized water and filtering, and repeating the whole step three times;
[0022] 4) placing the loofah powder obtained in step 3) into a 10% KOH aqueous solution at a material-liquid ratio of 1 g:20 mL to 1 g:50 mL, alkali washing at 80° C. for 4 to 6 h, cooling and washing with water until neutral, and filtering;
[0023] 5) placing the loofah powder obtained in step 4) into a 50% to 60% H2SO4 aqueous solution according to a material-liquid ratio of 1g:20mL to 1g:50mL, acid washing at 50°C for 6 to 8h, washing with water to neutrality after cooling, and centrifuging to neutrality;
[0024] 6) subjecting the cellulose aqueous solution obtained in step 5) to ultrasonic treatment in a cell disruptor at a power of 60 to 200 W for 1 to 3 hours;
[0025] 7) placing the cellulose aqueous solution obtained in step 6) into a freeze dryer and drying it at a temperature below -40°C for 20 to 40 hours to prepare loofah cellulose.
[0026] Compared with existing materials and technologies, the present invention has the following advantages and beneficial effects:
[0027] The 3D printing silicon carbide slurry of the present invention can be applied to ink direct writing 3D printers, and the printing height can exceed one centimeter. During the printing process, the slurry has the characteristics of stable extrusion speed, uniform density, not easy to break the wire, stable structure and not easy to collapse. Luffa cellulose is evenly dispersed in the silicon carbide particles as a dispersant. During the sintering process, the cellulose can be carbonized to connect the silicon carbide particles to increase the strength, and at the same time, the overall conductivity can be improved. The printed porous silicon carbide has good electromagnetic shielding performance and controllable thermal conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a real picture of the loofah cellulose after the freeze-drying step in Example 1.
[0029] Figure 2 This is the aqueous dispersion of low-concentration loofah cellulose in Example 1 and a picture showing the Tyndall effect.
[0030] Figure 3 This is the Zeta potential picture of the aqueous dispersion of low-concentration loofah cellulose in Example 1.
[0031] Figure 4 This is a scanning electron micrograph of the loofah cellulose in Example 1.
[0032] Figure 5 This is a transmission electron micrograph of the loofah cellulose in Example 1.
[0033] Figure 6The following are actual pictures of the dispersibility of loofah cellulose at different concentrations on silicon carbide in Example 1.
[0034] Figure 7 This is the Zeta potential picture of the 10 g / L loofah cellulose dispersion in Example 1.
[0035] Figure 8 This is the Zeta potential picture of the 20 g / L loofah cellulose dispersion in Example 1.
[0036] Fig. 9 This is a physical picture of the silicon carbide slurry prepared in Example 1 after 3D printing using ink direct writing technology.
[0037] Fig.10 Actual pictures of the 3D printed samples prepared in Examples 1(a), 2(b) and Comparative Example 1(c).
[0038] Fig.11 This is a macroscopic scanning electron micrograph of the 3D printed sample obtained in Example 1 after being heated at 1600°C for 2 hours.
[0039] Fig.12 This is a microscopic scanning electron micrograph of the 3D printed sample obtained in Example 1 after being heated at 1600°C for 2 hours.
[0040] Fig.13 This is a resistivity picture of the 3D printed sample obtained in Example 1 after being kept at 1600°C for 2 hours.
[0041] Fig.14 This is a picture of the electromagnetic shielding performance of the 3D printed sample prepared in Example 1 after being kept at 1600°C for 2 hours, including (a) electromagnetic shielding performance value and (b) shielding coefficient.
[0042] Fig.15 This is a picture of the density and thermal conductivity of the 3D printed sample prepared in Example 3 after being kept at 1600°C for 2 hours. DETAILED DESCRIPTION
[0043] Embodiment 1:
[0044] A 3D printing silicon carbide slurry suitable for ink direct writing technology comprises, by mass percentage, 40-60wt.% of silicon carbide ceramic powder, 0.3-1wt.% of loofah cellulose, 10-15wt.% of glycerol, 0.05-0.1wt.% of carrageenan, and the balance of deionized water.
[0045] The raw materials used mainly include silicon carbide powder (average particle size 600nm), loofah, benzene, anhydrous ethanol, sodium chlorite, glacial acetic acid, potassium hydroxide, concentrated sulfuric acid, glycerin, and carrageenan. The specific preparation process is as follows:
[0046] (1) Deionized water and glycerol are mixed in a volume ratio of 2:1 to obtain a water-oil mixture.
[0047] (2) Luffa cellulose and carrageenan were placed in a water-oil mixture at a material-liquid ratio of 10 g:1 L and 2 g:1 L, respectively, stirred at 80 °C for 30 min, and cooled to room temperature.
[0048] (3) The silicon carbide ceramic powder was mixed with the solution obtained in step (2) in a mass ratio of 2:1 and stirred at a stirring speed of 100 rpm for 1.0 h. The obtained slurry was filtered through a 2000 mesh screen. Fig. 9 and 10 (a) shown.
[0049] (4) The obtained porous silicon carbide sample was sintered at 1600°C for 2 hours under atmosphere protection. The microstructure of the sample after sintering is as follows: Figure 11-12 shown.
[0050] Wherein, the preparation method of loofah cellulose is:
[0051] 1) Raw material pretreatment: After washing the loofah, dry it at 80-90° C. for 4 h, grind it and pass it through a 40-mesh sieve to obtain loofah powder.
[0052] 2) Prepare a benzene-ethanol solution at a volume ratio of 2:1, wrap the loofah powder with filter paper, put it into a Soxhlet extractor at a solid-liquid ratio of 1g:20mL, and extract it at 100°C for 12 hours. After cooling naturally to room temperature, wash it with deionized water for 5 times and filter it.
[0053] 3) The loofah powder obtained in step 2) was placed in a 25 g / L NaClO2 aqueous solution according to a material-liquid ratio of 1 g:20 mL, the pH value was adjusted to 3 with glacial acetic acid, bleached at 80° C. for 3 h, cooled naturally to room temperature, washed with deionized water and filtered, and the whole step was repeated three times.
[0054] 4) The loofah powder obtained in step 3) was placed in a 10% KOH aqueous solution at a material-liquid ratio of 1 g:20 mL, and alkali washed at 80° C. for 5 h. After cooling, the powder was washed with water until neutral, and filtered.
[0055] 5) The loofah powder obtained in step 4) was placed in a 60% H2SO4 aqueous solution at a material-liquid ratio of 1 g:20 mL, acid-washed at 50° C. for 7 h, washed with water until neutral after cooling, and washed by centrifugation until neutral.
[0056] 6) The cellulose aqueous solution obtained in step 5) was ultrasonicated in a cell disruptor at a power of 150 W for 3 h.
[0057] 7) placing the cellulose aqueous solution obtained in step 6) into a freeze dryer and drying at a temperature below -40°C for 48 hours to prepare loofah cellulose, such as Figure 1-5 shown.
[0058] The prepared silicon carbide slurry is suitable for ink direct writing 3D printers, and the printing height can exceed one centimeter. During the printing process, the slurry has the characteristics of stable extrusion speed, uniform density, not easy to break the wire, stable structure and not easy to collapse. Luffa cellulose can well disperse silicon carbide ( Figure 6-8 ), and as a dispersant, it is evenly dispersed in the silicon carbide particles. During the sintering process, the carbonized cellulose can connect the silicon carbide particles to improve the strength, and at the same time improve the overall conductivity, such as Fig.13 As shown. The printed porous silicon carbide has good electromagnetic shielding performance ( Fig.14 ) and controllable thermal conductivity ( Fig.15 ).
[0059] Embodiment 2:
[0060] A 3D printing silicon carbide slurry suitable for ink direct writing technology, the raw materials used mainly include silicon carbide powder (average particle size 600nm), loofah, benzene, anhydrous ethanol, sodium chlorite, glacial acetic acid, potassium hydroxide, concentrated sulfuric acid, glycerin, and carrageenan. The specific preparation process is as follows:
[0061] (1) Deionized water and glycerol are mixed in a volume ratio of 2:1 to obtain a water-oil mixture.
[0062] (2) Luffa cellulose and carrageenan were placed in a water-oil mixture at a material-liquid ratio of 20 g:1 L and 2 g:1 L, respectively, stirred at 80 °C for 30 min, and cooled to room temperature.
[0063] (3) The silicon carbide ceramic powder was mixed with the solution obtained in step (2) in a mass ratio of 2:1 and stirred at a stirring speed of 100 rpm for 1.0 h. The obtained slurry was filtered through a 2000 mesh screen. Fig.10 (b) as shown.
[0064] (4) The obtained porous silicon carbide sample is sintered at 1600°C for 2 hours under atmosphere protection.
[0065] Wherein, the preparation method of loofah cellulose is:
[0066] 1) Raw material pretreatment: After washing the loofah, dry it at 80-90° C. for 6 h, grind it and pass it through a 40-mesh sieve to obtain loofah powder.
[0067] 2) Prepare a benzene-ethanol solution at a volume ratio of 2:1, wrap the loofah powder with filter paper, put it into a Soxhlet extractor at a solid-liquid ratio of 1g:20mL, and extract it at 100°C for 12 hours. After cooling naturally to room temperature, wash it with deionized water for 5 times and filter it.
[0068] 3) The loofah powder obtained in step 2) was placed in a 25 g / L NaClO2 aqueous solution according to a material-liquid ratio of 1 g:20 mL, the pH value was adjusted to 3 with glacial acetic acid, bleached at 80° C. for 3 h, cooled naturally to room temperature, washed with deionized water and filtered, and the whole step was repeated three times.
[0069] 4) The loofah powder obtained in step 3) was placed in a 10% KOH aqueous solution at a material-liquid ratio of 1 g:20 mL, and alkali washed at 80° C. for 5 h. After cooling, the powder was washed with water until neutral, and filtered.
[0070] 5) The loofah powder obtained in step 4) was placed in a 60% H2SO4 aqueous solution at a material-liquid ratio of 1 g:20 mL, acid-washed at 50° C. for 7 h, washed with water until neutral after cooling, and washed by centrifugation until neutral.
[0071] 6) The cellulose aqueous solution obtained in step 5) was ultrasonicated in a cell disruptor at a power of 200 W for 2 h.
[0072] 7) The cellulose aqueous solution obtained in step 6) is placed in a freeze dryer and dried at a temperature below -40°C for 48 hours to prepare loofah cellulose.
[0073] Embodiment 3:
[0074] A 3D printing silicon carbide slurry suitable for ink direct writing technology, the raw materials used mainly include silicon carbide powder (average particle size 600nm), loofah, benzene, anhydrous ethanol, sodium chlorite, glacial acetic acid, potassium hydroxide, concentrated sulfuric acid, glycerin, and carrageenan. The specific preparation process is as follows:
[0075] (1) Deionized water and glycerol were mixed in a volume ratio of 3:1 to obtain a water-oil mixture.
[0076] (2) Loofah cellulose and carrageenan were placed in a water-oil mixture at a material-liquid ratio of 50 g:1 L and 2 g:1 L, respectively, stirred at 80 °C for 30 min, and cooled to room temperature.
[0077] (3) The silicon carbide ceramic powder and the solution obtained in step (2) were mixed and stirred at a mass ratio of 2:1 at a stirring speed of 100 rpm for 1.0 h, and the obtained slurry was filtered through a 2000 mesh sieve.
[0078] (4) The obtained porous silicon carbide sample is sintered at 1600°C for 2 hours under atmosphere protection.
[0079] Wherein, the preparation method of loofah cellulose is:
[0080] 1) Raw material pretreatment: After washing the loofah, dry it at 80-90° C. for 6 h, grind it and pass it through a 40-mesh sieve to obtain loofah powder.
[0081] 2) Prepare a benzene-ethanol solution at a volume ratio of 2:1, wrap the loofah powder with filter paper, put it into a Soxhlet extractor at a solid-liquid ratio of 1g:20mL, and extract it at 100°C for 12 hours. After cooling naturally to room temperature, wash it with deionized water for 5 times and filter it.
[0082] 3) The loofah powder obtained in step 2) was placed in a 25 g / L NaClO2 aqueous solution according to a material-liquid ratio of 1 g:20 mL, the pH value was adjusted to 3 with glacial acetic acid, bleached at 80° C. for 3 h, cooled naturally to room temperature, washed with deionized water and filtered, and the whole step was repeated three times.
[0083] 4) The loofah powder obtained in step 3) was placed in a 10% KOH aqueous solution at a material-liquid ratio of 1 g:20 mL, and alkali washed at 80° C. for 5 h. After cooling, the powder was washed with water until neutral, and filtered.
[0084] 5) The loofah powder obtained in step 4) was placed in a 60% H2SO4 aqueous solution at a material-liquid ratio of 1 g:20 mL, acid-washed at 50° C. for 7 h, washed with water until neutral after cooling, and washed by centrifugation until neutral.
[0085] 6) The cellulose aqueous solution obtained in step 5) was ultrasonicated in a cell disruptor at a power of 200 W for 2 h.
[0086] 7) The cellulose aqueous solution obtained in step 6) is placed in a freeze dryer and dried at a temperature below -40°C for 48 hours to prepare loofah cellulose.
[0087] Comparative Example 1:
[0088] The main difference between Comparative Example 1 and Examples 1, 2, and 3 is that no loofah cellulose is added to the prepared slurry, as follows:
[0089] A 3D printing silicon carbide slurry comprises, by weight percentage, 40-60 wt.% of silicon carbide ceramic powder, 10-15 wt.% of glycerol, 0.05-0.1 wt.% of carrageenan, and the balance of deionized water.
[0090] (1) Deionized water and glycerol are mixed in a volume ratio of 2:1 to obtain a water-oil mixture.
[0091] (2) Carrageenan was added into the water-oil mixture at a solid-liquid ratio of 2 g:1 L, stirred at 80 °C for 30 min, and cooled to room temperature.
[0092] (3) The silicon carbide ceramic powder was mixed with the solution obtained in step (2) in a mass ratio of 2:1 and stirred at a stirring speed of 100 rpm for 1.0 h. The obtained slurry was filtered through a 2000 mesh screen. Fig.10 (c) as shown.
[0093] (4) The obtained porous silicon carbide sample is sintered at 1600°C for 2 hours under atmosphere protection.
[0094] The resistivities of the samples prepared with cellulose contents of 0 g / L (Comparative Example 1), 10 g / L (Example 1), 20 g / L (Example 2), and 50 g / L (Example 3) in the solution were 658.61 kΩ·cm, 495.26 kΩ·cm, 360.55 kΩ·cm, and 8.82 kΩ·cm, respectively.
[0095] Matters not covered by the present invention are known technologies.
[0096] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing silicon carbide slurry for 3D printing suitable for ink direct writing technology, characterized in that: The slurry is composed of: 40-60wt.% silicon carbide ceramic powder, 0.3-1wt.% loofah cellulose, 10-15wt.% glycerol, 0.05-0.1wt.% carrageenan, and the balance is deionized water; the silicon carbide ceramic powder is silicon carbide whiskers and / or silicon carbide particles, and its particle size is 50nm-50μm, and its purity is 99%-99.99%; the loofah cellulose is filamentous or flaky, and its size ranges from 10nm to 1μm; The following steps are involved: (1) Mixing deionized water and glycerol in a volume ratio of 2:1 to 1:1 to obtain a water-oil mixture; (2) Add loofah cellulose and carrageenan into a water-oil mixture at a material-liquid ratio of 10-50 g:1 L and 2-5 g:1 L, respectively, stir at 80 °C for 30 min, and cool to room temperature; (3) Mix the silicon carbide ceramic powder with the solution obtained in step (2) in a mass ratio of 3:1 to 2:1, and filter the obtained slurry through a 2000-mesh sieve.
2. The method for preparing silicon carbide slurry for 3D printing suitable for ink direct writing technology according to claim 1, characterized in that: In step (3), the mixing process of silicon carbide ceramic powder and solution is stirring and / or ball milling; wherein: The stirring speed is 10-500 rpm, and the stirring time is greater than 0.5 h; The ball milling speed is 30-300 rpm, the ball milling time is 4-10 hours, and the mass ratio of the grinding balls to the slurry is greater than 0.
1.
3. The method for preparing silicon carbide slurry for 3D printing suitable for ink direct writing technology according to claim 1, characterized in that: The preparation method of the loofah cellulose is: 1) Raw material pretreatment: After washing the loofah, dry it at 80-90°C for 4-6 hours, crush it and pass it through a 40-mesh sieve to obtain loofah powder; 2) Prepare benzene-ethanol solution at a volume ratio of 2:1, wrap the loofah powder with filter paper, put it into a Soxhlet extractor at a solid-liquid ratio of 1g:20mL~1g:50mL, and extract at 80℃~100℃ for 6~12h; after cooling naturally to room temperature, wash with deionized water 4~6 times, and filter; 3) Put the loofah powder obtained in step 2) into a 20g / L~30g / L NaClO2 aqueous solution according to a material-liquid ratio of 1g:20mL~1g:50mL, adjust the pH value to 2~3 with glacial acetic acid, bleach at 80℃ for 2~4h, cool naturally to room temperature, wash with deionized water and filter, and repeat the whole step three times; 4) Put the loofah powder obtained in step 3) into a 10% KOH aqueous solution at a material-liquid ratio of 1g:20mL~1g:50mL, perform alkali washing at 80℃ for 4~6h, wash with water until neutral after cooling, and filter; 5) Put the loofah powder obtained in step 4) into a 50% to 60% H2SO4 aqueous solution according to a material-liquid ratio of 1g:20mL to 1g:50mL, acid wash at 50°C for 6 to 8h, wash with water until neutral after cooling, and centrifuge and wash until neutral; 6) ultrasonicating the cellulose aqueous solution obtained in step 5) in a cell disruptor at a power of 60-200 W for 1-3 h; 7) The cellulose aqueous solution obtained in step 6) is placed in a freeze dryer and dried for 20 to 40 hours to prepare loofah cellulose.
4. The method for preparing silicon carbide slurry for 3D printing suitable for ink direct writing technology according to claim 3, characterized in that: In step 7), the temperature in the freeze dryer is lower than -40°C.