Lubricating microcapsule and preparation method thereof and self-lubricating composite material

By combining solid and liquid lubricants in lubricating microcapsules and using dispersants and surfactants, the use temperature range of lubricating microcapsules is expanded, and the problem of failure of lubricating microcapsules in the previous technology is solved, and the problem of lubricating microcapsules in the wide temperature domain is achieved. Good lubrication performance between -50 and 400°C.

CN116240065BActive Publication Date: 2024-11-12TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211593063.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-12
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Existing lubricated microcapsules fail under low and high temperature conditions and cannot provide good lubricating performance in a wide temperature range.

Method used

Using a core material including solid lubricant, liquid lubricant and dispersant, combined with shell components such as surfactants and emulsifiers, the use temperature range of lubricating microcapsules is expanded by mechanical stirring or ultrasonic mixing. .

Benefits of technology

The lubricated microcapsules have achieved good lubricating performance in a wide temperature range of -50~400℃, which has expanded its application range in industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116240065B_ABST
    Figure CN116240065B_ABST
Patent Text Reader

Abstract

The present invention provides a lubricating microcapsule, comprising a core material and a shell layer coated on the outside of the core material; the components of the core material include a solid lubricant, a liquid lubricant and a dispersant; the components of the shell layer include a shell material, a surfactant and an emulsifier. By compounding the solid lubricant into the liquid lubricant, the lubricating microcapsule can still have good lubrication performance at low and high temperatures, broadening the use temperature range of the lubricating microcapsule, so that it has a wide temperature range lubrication performance, expanding the application field of the lubricating microcapsule in industry, and the application method is more flexible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lubricants, in particular to a lubricating microcapsule and a preparation method thereof and a self-lubricating composite material. Background Art

[0002] Microcapsule technology refers to a micro-packaging technology that encapsulates trace substances in polymer films to store solids, liquids, and gases. Microcapsules are increasingly being used to adjust or enhance the lubrication properties of materials.

[0003] At present, the main structure of lubricating microcapsules is lubricating oil core material, organic, inorganic or organic / inorganic composite shell material. These microcapsules are mainly used for lubrication at room temperature and some medium temperature conditions. As the temperature drops to -50℃ or even lower, the viscosity of the lubricating oil core material will gradually increase until it solidifies, thus losing the lubricating effect. As the temperature rises, after exceeding the evaporation temperature of the lubricating oil, the lubricating oil core material will gradually evaporate, and the lubricating effect will also be lost. Summary of the invention

[0004] Based on this, it is necessary to provide a lubricating microcapsule and a preparation method thereof and a self-lubricating composite material that can be used under a wide temperature range.

[0005] A first aspect of the present invention provides a lubricating microcapsule, comprising:

[0006] A core material, wherein the components of the core material include a solid lubricant, a liquid lubricant and a dispersant;

[0007] The shell layer is coated on the outside of the core material, and the components of the shell layer include shell material, surfactant and co-emulsifier.

[0008] In some embodiments, the lubricating microcapsules satisfy at least one of the following conditions:

[0009] (1) The particle size of the lubricating microcapsules is 0.1 to 100 μm;

[0010] (2) The mass ratio of the core material to the shell layer in the lubricating microcapsule is (2-4):5;

[0011] (3) The friction coefficient of the lubricating microcapsules is 0.04 to 0.1;

[0012] (4) The operating temperature range of the lubricating microcapsules is -50 to 400°C.

[0013] In some embodiments, the core material comprises at least one of the following conditions:

[0014] (1) The mass ratio of the solid lubricant to the liquid lubricant is 1:(2-100);

[0015] (2) The mass of the dispersant accounts for 0.1 to 10% of the total mass of the solid lubricant and the liquid lubricant;

[0016] (3) The solid lubricant includes one or more of molybdenum disulfide, tungsten disulfide, graphene, fullerene, black phosphorus, purple phosphorus, magnesium hydroxysilicate, titanium carbide, nano-gold, nano-silver, nano-copper, nano-nickel, nano-iron, nano-zinc, nano-copper oxide, nano-aluminum oxide, nano-zinc oxide and nano-zirconium oxide; preferably one or more of molybdenum disulfide and tungsten disulfide;

[0017] (4) The liquid lubricant includes one or more of an oil-soluble ionic liquid and a lubricating oil;

[0018] Optionally, the oil-soluble ionic liquid includes one or more of 1-butyl-3-methylimidazolium hexafluorophosphate, 1-octyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-methyl-3-n-octyl imidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-ethyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt and 1-octyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt; preferably 1-butyl-3-methylimidazolium hexafluorophosphate;

[0019] Optionally, the lubricating oil includes one or more of hydrogenated polydecene, linseed oil, alkyl silicone oil, phenyl silicone oil, chain oil, tung oil, mineral oil, ester base oil, liquid paraffin, perfluoropolyether, heavy alkylbenzene and oleic acid; preferably one or more of hydrogenated polydecene, heavy alkylbenzene and phenyl silicone oil;

[0020] (5) The dispersant includes one or more of Span 80 and boronated polyisobutylene succinimide.

[0021] In some embodiments, the shell comprises at least one of the following conditions:

[0022] (1) The mass ratio of the surfactant to the co-emulsifier is (0.1-5):(0.1-5);

[0023] (2) The shell material includes one or more of silicon dioxide and urea-formaldehyde resin;

[0024] (3) The surfactant comprises one or more of polyvinyl alcohol, Triton X100, Tween 80, sodium dodecylbenzene sulfonate, ammonium dodecyl sulfate, hexadecyltrimethylammonium bromide, gelatin, gum arabic and lignin; preferably one or more of polyvinyl alcohol, Triton X100, Tween 80 and gum arabic;

[0025] (4) The co-emulsifier includes one or more of n-butanol, ethylene glycol, n-hexadecane, propylene glycol, glycerol and polyglycerol ester; preferably n-hexadecane.

[0026] The present invention also provides a method for preparing lubricating microcapsules, comprising the following steps:

[0027] Mixing the solid lubricant, the liquid lubricant and the dispersant to obtain a core material;

[0028] Mixing the surfactant, the co-emulsifier and the solvent A to obtain phase A, and adjusting the pH value of phase A;

[0029] Mixing the shell material precursor and solvent B to obtain phase B;

[0030] The core material, the phase A and the phase B are mixed and reacted, and the reaction product is dried to obtain the lubricating microcapsules.

[0031] In some embodiments, when preparing the core material, mechanical stirring or ultrasound is used to mix the solid lubricant, the liquid lubricant and the dispersant;

[0032] Optionally, the mechanical stirring rate is 100 to 2000 rpm, and the mechanical stirring time is 10 to 20 min;

[0033] Optionally, the ultrasonic power is 50 to 1200 W, and the ultrasonic time is 10 to 120 min.

[0034] In some embodiments, the preparation of the phase A includes at least one of the following conditions:

[0035] (1) The mass percentage of the surfactant in the phase A is 0.1 to 5%;

[0036] (2) The mass proportion of the co-emulsifier in the phase A is 0.1 to 5%;

[0037] (3) The pH value of phase A is 2 to 12;

[0038] (4) The solvent A includes water.

[0039] In some embodiments, the preparation of the phase B includes at least one of the following conditions:

[0040] (1) The precursor of the shell material includes tetraethyl orthosilicate or a mixture of urea, formaldehyde and resorcinol or a mixture of tetraethyl orthosilicate, urea, formaldehyde and resorcinol;

[0041] (2) The mass proportion of the precursor of the shell material in the B phase is 0.2 to 40%;

[0042] (3) The solvent B is water or a mixture of ethanol and water.

[0043] In some embodiments, the step of mixing the core material, the phase A and the phase B for reaction specifically comprises:

[0044] Add the core material into the phase A and disperse it;

[0045] Adding the phase B into the phase A to obtain a mixed solution, and reacting the mixed solution at 10-100° C. for 30-480 min;

[0046] Optionally, the process used when dispersing the core material and the phase A includes: stirring at a stirring rate of 100 to 2000 rpm for 5 to 60 minutes or ultrasonicating at an ultrasonic power of 50 to 1200 W for 5 to 60 minutes;

[0047] Optionally, when the phase B is added to the phase A, the phase A is stirred at a stirring rate of 100 to 2000 rpm or ultrasonicated at an ultrasonic power of 50 to 1200 W.

[0048] The present invention also provides a self-lubricating composite material, comprising the lubricating microcapsules or the lubricating microcapsules prepared by the above method.

[0049] The lubricating microcapsules, preparation methods thereof and self-lubricating composite materials provided above, by compounding solid lubricants into liquid lubricants, enable the lubricating microcapsules to still have good lubrication properties at low and high temperatures, thereby broadening the use temperature range of the lubricating microcapsules, thereby giving them wide-temperature range lubrication properties, expanding the application fields of the lubricating microcapsules in industry, and making the application methods more flexible. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is a schematic diagram of the scanning electron microscope of the HAB / WS2@SiO2 microcapsule in Example 1;

[0051] Figure 2 Schematic diagram of transmission electron microscopy of HAB / WS2@SiO2 microcapsules in Example 1;

[0052] Figure 3 This is a schematic diagram of an optical microscope of the HAB / WS2@SiO2 microcapsule in Example 1;

[0053] Figure 4 This is a schematic diagram of the scanning electron microscope of PAO6 / MoS2@UF microcapsules in Example 2;

[0054] Figure 5 Schematic diagram of the change of the friction coefficient of the self-lubricating composite material block over time in Example 1 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0055] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0056] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0057] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0058] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0059] In this article, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 15-17 shares means that the units of the left endpoint "15" and the right endpoint "17" are both shares.

[0060] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0061] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.

[0062] In addition, in the description of the invention, “plurality” means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.

[0063] If there is no special description, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.

[0064] If there is no special explanation, all the steps of the present application can be performed sequentially or randomly, preferably sequentially.

[0065] The invention provides a lubricating microcapsule, comprising: a core material and a shell layer coated on the outside of the core material; the components of the core material include solid lubricant, liquid lubricant and dispersant; the components of the shell layer include shell material, surfactant and emulsifier.

[0066] It should be noted that liquid lubricant refers to a lubricant that is in a liquid state within its operating temperature range; solid lubricant refers to a lubricant that is in a solid state within its operating temperature range.

[0067] In the present invention, by using a solid lubricant, a liquid lubricant and a dispersant in combination, the solid lubricant can be uniformly dispersed in the liquid lubricant under the action of the dispersant, and in the preparation process of the lubricating microcapsules, the dispersant can prevent the solid lubricant from separating from the liquid lubricant and entering the water phase. If the dispersant is not used when preparing the core material, it is impossible to prepare a lubricating microcapsule containing both the solid lubricant and the liquid lubricant as the core material.

[0068] Understandably, by compounding the solid lubricant into the liquid lubricant, the lubricating microcapsules can still have good lubrication properties at low and high temperatures, broadening the operating temperature range of the lubricating microcapsules, thereby giving them wide-temperature range lubrication properties, expanding the application areas of the lubricating microcapsules in industry, and making the application methods more flexible.

[0069] In some embodiments, the particle size of the lubricating microcapsules is 0.1 to 100 μm; for example, it can be 1 to 100 μm, 1 to 90 μm, 1 to 80 μm, 1 to 70 μm, 1 to 60 μm, 1 to 50 μm, 1 to 40 μm, 10 to 40 μm, 10 to 30 μm or 10 to 20 μm, etc., without specific limitation.

[0070] In some embodiments, the mass ratio of the core material to the shell layer in the lubricating microcapsule is (2-4):5; for example, it can be 2:5, 2.5:5, 3:5, 3.5:5, 4:5 or 4.5:5, etc., without specific limitation.

[0071] In some embodiments, the friction coefficient of the lubricating microcapsules is 0.04 to 0.1; for example, it can be 0.04 to 0.09, 0.05 to 0.08, 0.05 to 0.0.07 or 0.05 to 0.06, etc., without specific limitation. Compared with the core material containing only liquid lubricants or solid lubricants, when the core material contains both liquid lubricants and solid lubricants, the friction coefficient of the lubricating microcapsules can be significantly reduced. This is because during the friction process, as the microcapsules rupture, the liquid lubricant will be released to form a lubricating film between the grinding pair interfaces, and the solid lubricant carried therein will therefore be evenly dispersed between the grinding pairs. In addition, the synergistic lubrication effect between the solid lubricant and the liquid lubricant can further reduce the friction coefficient.

[0072] In some embodiments, the operating temperature range of the lubricating microcapsules is -50 to 400°C; for example, it can be -20 to 400°C, -20 to 380°C, 0 to 350°C, 50 to 300°C, 100 to 250°C, 150 to 200°C or -50 to 300°C, etc., without specific limitation. Compared with the core material containing only liquid lubricants or solid lubricants, when the core material contains both liquid lubricants and solid lubricants, the operating temperature of the lubricating microcapsules can be effectively widened, and in particular, the minimum operating temperature of the lubricating microcapsules can be reduced. This is because although the liquid lubricant solidifies at a use temperature of -50°C, the liquid lubricant in the lubricating microcapsules evenly disperses the solid lubricant during the friction process. Therefore, when the use temperature is -50°C, the solid lubricant can be evenly dispersed at the friction interface, and the solid lubricant can still play a good lubricating effect at low temperatures.

[0073] In some embodiments, the mass ratio of the solid lubricant to the liquid lubricant in the core material is 1:(2-100); for example, it can be 1:(5-100), 1:(5-95), 1:(10-90), 1:(15-85), 1:(20-80), 1:(25-75), 1:(30-70), 1:(35-65), 1:(40-60), 1:(45-55), 1:(50-55) or 1:(2-90), etc., and is not specifically limited. When the mass ratio of the solid lubricant to the liquid lubricant in the core material is within the above range, the viscosity of the liquid lubricant is not too large to be unable to be coated, and the content of the solid lubricant is not too low to be unable to play a synergistic lubricating role; when the amount of the solid lubricant is too small, the friction coefficient of the lubricating microcapsule increases; when the amount of the solid lubricant is too much, the viscosity of the core material increases, which will cause the particle size of the lubricating microcapsule to increase.

[0074] In some embodiments, the mass ratio of the dispersant in the core material to the total mass of the solid lubricant and the liquid lubricant is 0.1-10%; for example, it can be 0.5-10%, 0.5-9.5%, 1-9%, 1.5-8.5%, 2-8%, 2.5-7.5%, 3-7%, 3.5-6.5%, 4-6%, 4.5-5.5%, 5-5.5% or 0.1-9%, etc., and is not specifically limited. When the mass ratio of the dispersant in the core material to the total mass of the solid lubricant and the liquid lubricant is within the above range, it can ensure that the solid lubricant is uniformly dispersed without affecting the performance of the solid-liquid composite lubricant.

[0075] In some embodiments, the solid lubricant in the core material includes one or more of molybdenum disulfide, tungsten disulfide, graphene, fullerene, black phosphorus, purple phosphorus, magnesium hydroxysilicate, titanium carbide, nano-gold, nano-silver, nano-copper, nano-nickel, nano-iron, nano-zinc, nano-copper oxide, nano-aluminum oxide, nano-zinc oxide, and nano-zirconium oxide. Preferably, one or more of molybdenum disulfide and tungsten disulfide are used.

[0076] In some embodiments, the liquid lubricant in the core material includes one or more of an oil-soluble ionic liquid and a lubricating oil.

[0077] Optionally, the oil-soluble ionic liquid includes one or more of 1-butyl-3-methylimidazolium hexafluorophosphate, 1-octyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-methyl-3-n-octyl imidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-ethyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt and 1-octyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt. Preferably, 1-butyl-3-methylimidazolium hexafluorophosphate is used.

[0078] Optionally, the lubricating oil includes one or more of hydrogenated polydecene, linseed oil, alkyl silicone oil, phenyl silicone oil, chain oil, tung oil, mineral oil, ester base oil, liquid paraffin, perfluoropolyether, heavy alkyl benzene and oleic acid. Preferably, it is one or more of hydrogenated polydecene, heavy alkyl benzene and phenyl silicone oil.

[0079] In some embodiments, the dispersant includes one or more of Span 80 and boronated polyisobutylene succinimide.

[0080] In some embodiments, the mass ratio of the surfactant to the co-emulsifier in the shell layer is (0.1-5):(0.1-5).

[0081] In some embodiments, the shell material in the shell layer includes one or more of silica and urea-formaldehyde resin.

[0082] In some embodiments, the surfactant in the shell layer includes one or more of polyvinyl alcohol, Triton X100, Tween 80, sodium dodecylbenzene sulfonate, ammonium dodecyl sulfate, hexadecyltrimethylammonium bromide, gelatin, gum arabic and lignin, preferably one or more of polyvinyl alcohol, Triton X100, Tween 80 and gum arabic.

[0083] In some embodiments, the co-emulsifier in the shell layer includes one or more of n-butanol, ethylene glycol, n-hexadecane, propylene glycol, glycerol and polyglycerol esters, preferably n-hexadecane.

[0084] The present invention also provides a method for preparing lubricating microcapsules, comprising the following steps:

[0085] The solid lubricant, the liquid lubricant and the dispersant are mixed to obtain a core material;

[0086] Mixing the surfactant, the co-emulsifier and the solvent A to obtain phase A, and adjusting the pH value of phase A;

[0087] Mixing the shell material precursor and solvent B to prepare phase B;

[0088] The core material, phase A and phase B are mixed and reacted, and the reaction product is dried to obtain lubricating microcapsules.

[0089] In some embodiments, when preparing the core material, the solid lubricant, the liquid lubricant and the dispersant are mixed by mechanical stirring or ultrasound.

[0090] Optionally, when mechanical stirring is used to mix the solid lubricant, liquid lubricant and dispersant, the mechanical stirring rate is 100-2000rpm; for example, it can be 200-2000rpm, 200-1800rpm, 400-1600rpm, 600-1400rpm, 800-1200rpm, 1000-1200rpm or 200-1500rpm, etc., without specific limitation. The mechanical stirring time is 10-20min; for example, it can be 11-20min, 11-19min, 12-18min, 13-17min, 14-16min, 15-16min or 10-15min, etc., without specific limitation. When the mechanical stirring rate and mechanical stirring time are set in the above ranges, it can ensure that the solid lubricant is evenly dispersed in the liquid lubricant without agglomeration or the appearance of larger particles.

[0091] Optionally, when ultrasonic mixing of solid lubricants, liquid lubricants and dispersants is used, the ultrasonic power is 50 to 1200 W; for example, it can be 100 to 1200 W, 100 to 1100 W, 200 to 1000 W, 300 to 900 W, 400 to 800 W, 500 to 700 W, 500 to 600 W, or 50 to 1000 W, etc., without specific limitation. The ultrasonic time is 10 to 20 min; for example, it can be 11 to 20 min, 11 to 19 min, 12 to 18 min, 13 to 17 min, 14 to 16 min, 15 to 16 min or 10 to 15 min, etc., without specific limitation. When the ultrasonic power and ultrasonic time are respectively set in the above ranges, it can ensure that the solid lubricant is evenly dispersed in the liquid lubricant without agglomeration or the appearance of larger particles.

[0092] In some embodiments, when preparing phase A, the mass proportion of the surfactant in phase A is 0.1-5%; for example, it can be 0.3-5%, 0.3-4.5%, 0.5-4%, 1-3.5%, 1.5-3%, 2-3%, 2-2.5% or 0.1-4%, etc., without specific limitation. When the mass proportion of the surfactant in phase A is within the above range, it can be mixed with phase B to obtain a stable oil-in-water (O / W) emulsion.

[0093] In some embodiments, when preparing phase A, the mass proportion of the co-emulsifier in phase A is 0.1-5%; for example, it can be 0.5-5%, 0.5-4.5%, 0.5-4%, 1-3.5%, 1.5-3%, 2-3%, 2-2.5% or 0.1-3.5%, etc., and is not specifically limited. When the mass proportion of the co-emulsifier in phase A is within the above range, a stable fine emulsion with droplets less than 10 μm can be obtained.

[0094] In some embodiments, the pH value of phase A is 2 to 12; for example, it can be 3 to 12, 3 to 11, 4 to 10, 5 to 9, 6 to 8, 7 to 8 or 2 to 11, etc., without specific limitation. When the pH value of phase A is within the above range, the conditions for the shell material precursor to react to form the shell material can be met; if the pH value of phase A is not within the above range, the precursor will not react or the reaction degree is low or the reaction rate is extremely slow.

[0095] In some embodiments, when preparing phase A, solvent A includes water. Alternatively, when preparing phase A, solvent A is water.

[0096] In some embodiments, when preparing phase B, the precursor of the shell material may include tetraethyl orthosilicate, or may include a mixture of urea, formaldehyde and resorcinol, or may include a mixture of tetraethyl orthosilicate, urea, formaldehyde and resorcinol.

[0097] It should be noted that, during the preparation of the lubricating microcapsules, ethyl orthosilicate undergoes a chemical reaction to generate silicon dioxide, and urea, formaldehyde and resorcinol undergo a chemical reaction to generate urea-formaldehyde resin. Optionally, when the precursor of the shell material contains formaldehyde, a formaldehyde aqueous solution with a solid content of 37% is used as a raw material for providing formaldehyde.

[0098] In some embodiments, when preparing phase B, the mass proportion of the precursor of the shell material in phase B is 0.2-40%; for example, it can be 0.5-40%, 0.5-39%, 1-35%, 5-35%, 10-30%, 15-25%, 20-25%, 15-20% or 0.2-30%, etc., without specific limitation. When the mass proportion of the precursor of the shell material in phase B is within the above range, microcapsules with moderate shell material thickness and intact morphology can be obtained.

[0099] In some embodiments, when preparing phase B, solvent B is water or a mixture of ethanol and water.

[0100] In the technical solution of the present invention, the volume ratio of ethanol to water in the solvent after the mixture of phase A and phase B is (0-1):1; for example, it can be (0.1-1):1, (0.2-0.9):1, (0.3-0.8):1, (0.4-0.7):1 or (0.5-0.6):1, etc., without specific limitation. It should be noted that when the volume ratio of ethanol to water is 0:1, it means that the solvent B is all water. When the volume ratio of ethanol to water is within the above range, the reaction conditions of the shell material precursor can be met; if there is too much ethanol, the reaction rate is too fast and microcapsules cannot be obtained.

[0101] In some embodiments, the step of mixing the core material, phase A and phase B for reaction specifically includes:

[0102] Add the core material into phase A and disperse;

[0103] Phase B is added to phase A to obtain a mixed solution, and the mixed solution is reacted at 10-100°C for 30-480 minutes. When the reaction temperature and reaction time are respectively within the above ranges, the reaction conditions of the precursor can be met; otherwise, the temperature is too low and no reaction occurs, and the temperature is too high and the reactants are destroyed.

[0104] Specifically, the process used to disperse the core material and phase A includes: stirring at a stirring rate of 100 to 2000 rpm for 5 to 60 minutes or ultrasonicating at an ultrasonic power of 50 to 1200 W for 5 to 60 minutes. When the core material and phase A are dispersed using the above process parameters, the stability of the emulsion can be maintained.

[0105] Optionally, when adding phase B to phase A, phase A is stirred at a stirring rate of 100 to 2000 rpm or ultrasonicated at an ultrasonic power of 50 to 1200 W. When adding phase B to phase A, stirring or ultrasonicating phase A can maintain the stability of the emulsion.

[0106] In some embodiments, the reaction product may be dried naturally at room temperature, or may be dried in an oven at 30 to 120°C.

[0107] The present invention also provides a self-lubricating composite material, comprising the lubricating microcapsules mentioned above or the lubricating microcapsules prepared in the above manner.

[0108] The technical solution of the present invention is described in detail below in conjunction with specific embodiments.

[0109] It should be noted that HAB mentioned in the following embodiments or comparative examples is heavy alkylbenzene, WS2 is tungsten disulfide, MoS2 is molybdenum disulfide, PA12 is nylon 12, [BMIM]PF6 is 1-butyl-3-methylimidazole hexafluorophosphate, and PAO6 is a type of hydrogenated polydecene.

[0110] 1. Preparation of Lubricating Microcapsules

[0111] Example 1

[0112] S1: 10 g HAB, 0.5 g WS2 and 0.5 g Span 80 were mixed and ultrasonicated at 100 W power for 10 min to obtain a core material;

[0113] S2: Take 1 g of polyvinyl alcohol, 0.5 g of gum arabic and 0.5 g of n-hexadecane, add them into 100 mL of deionized water, and stir at 100 °C until the polyvinyl alcohol and gum arabic are completely dissolved to obtain phase A, and adjust the pH value of phase A to 11 with ammonia water;

[0114] S3: Take 1 g of ethyl orthosilicate and dissolve it in 10 mL of 75% ethanol aqueous solution to obtain phase B;

[0115] S4: Add the core material to phase A and perform ultrasound at 50W power for 20 minutes. Transfer phase A to a three-necked flask. Add phase B to phase A while stirring phase A at a stirring rate of 600 rpm. Heat the reaction in a water bath at 45°C for 60 minutes.

[0116] S5: filtering the solution after the reaction to obtain a reaction product, washing the reaction product, and freeze-drying it to obtain HAB / WS2@SiO2 microcapsules.

[0117] Example 2

[0118] S1: 10 g PAO6, 0.5 g molybdenum disulfide and 0.5 g Span 80 were mixed and ultrasonicated at 100 W power for 20 min to obtain a core material;

[0119] S2: Take 1 g of polyvinyl alcohol, 0.5 g of gum arabic and 0.6 g of n-hexadecane, add them into 150 mL of deionized water, and stir at 100 °C until the polyvinyl alcohol and gum arabic are completely dissolved to obtain phase A, and adjust the pH value of phase A to 3 with 1 mol / L hydrochloric acid standard solution;

[0120] S3: Take 5 g of urea, 5 g of formaldehyde, and 0.5 g of resorcinol and dissolve them in 50 mL of deionized water to obtain phase B;

[0121] S4: Add the core material to phase A and stir at 2000 rpm for 30 min. Transfer phase A to a three-necked flask. Add phase B to phase A while stirring phase A at 1200 rpm. Heat in a water bath at 70°C for 240 min.

[0122] S5: filtering the solution after the reaction to obtain a reaction product, washing the reaction product, and freeze-drying it to obtain PAO6 / MoS2@UF microcapsules.

[0123] Example 3

[0124] S1: 1 g [BMIM]PF6, 0.5 g molybdenum disulfide, and 0.15 g boronated polyisobutylene succinimide were mixed and ultrasonicated at 1200 W power for 10 min to obtain a core material;

[0125] S2: Take 5 g of Triton X100 and 0.1 g of n-hexadecane, add them to 100 mL of deionized water, and stir at 100 °C until Triton X100 is completely dissolved to obtain phase A, and adjust the pH value of phase A to 2 with 1 mol / L hydrochloric acid standard solution;

[0126] S3: Take 5 g of urea, 5 g of formaldehyde, and 0.5 g of resorcinol and dissolve them in 50 mL of deionized water to obtain phase B;

[0127] S4: Add the core material to phase A and stir at 100 rpm for 60 min. Transfer phase A to a three-necked flask. Add phase B to phase A while stirring phase A at 100 rpm. Heat the mixture in a water bath at 100°C for 30 min.

[0128] S5: Filter the solution after the reaction to obtain the reaction product, wash the reaction product, and freeze-dry it to obtain [BMIM]PF6 / MoS2@UF microcapsules.

[0129] Example 4

[0130] S1: 50 g of phenyl silicone oil, 0.5 g of tungsten disulfide, and 0.05 g of Span 80 were mixed, and stirred at a stirring rate of 2000 rpm for 10 min to obtain a core material;

[0131] S2: Take 0.1 g of Tween 80 and 5 g of n-hexadecane, add them to 100 mL of deionized water, and stir at 100 °C until Triton X100 is completely dissolved to obtain phase A. Use 1 mol / L hydrochloric acid standard solution to adjust the pH value of phase A to 12;

[0132] S3: Take 5 g of urea, 5 g of formaldehyde, and 0.5 g of resorcinol and dissolve them in 50 mL of deionized water to obtain phase B;

[0133] S4: Add the core material to phase A and ultrasonicate at a power of 1200 W for 5 min. Transfer phase A to a three-necked flask. Add phase B to phase A while ultrasonicating phase A at a power of 1200 W. Heat the reaction in a water bath at 10°C for 480 min.

[0134] S5: filtering the solution after the reaction to obtain a reaction product, washing the reaction product, and freeze-drying it to obtain phenyl silicone oil / WS2@UF microcapsules.

[0135] Example 5

[0136] The difference between Example 5 and Example 1 is that the amounts of HAB and WS2 used are different, specifically: 10.4 g HAB, 0.104 g WS2, and the others are the same.

[0137] Example 6

[0138] The difference between Example 6 and Example 1 is that the amounts of HAB and WS2 are different, specifically 7 g HAB and 3.5 g WS2, and the others are the same.

[0139] Comparative Example 1

[0140] The difference between Comparative Example 1 and Example 1 is that WS2 is not added when preparing the core material, and HAB of the same mass is used to replace WS2. Other things are the same, and finally HAB@SiO2 microcapsules are prepared.

[0141] Comparative Example 2

[0142] Use WS2 of the same quality to replace HAB, and only use WS2.

[0143] Comparative Example 3

[0144] The difference between Comparative Example 3 and Example 1 is that Span 80 is not added when preparing the core material, and the other aspects are the same.

[0145] During the preparation process, the solid lubricant escapes from the liquid lubricant and enters the water-oil interface and cannot be retained in the liquid lubricant, so lubricating microcapsules cannot be prepared.

[0146] 2. Preparation of self-lubricating composite materials

[0147] 0.6 g of the lubricating microcapsules prepared in Examples 1 to 6 and Comparative Examples 1 to 2 and 5.4 g of PA12 powder were mixed in deionized water, stirred, filtered, and dried, and a self-lubricating composite material block was prepared by hot pressing and sintering.

[0148] 2. Performance Test

[0149] 1. The HAB / WS2@SiO2 microcapsules prepared in Example 1 were observed using scanning electron microscopy, transmission electron microscopy and optical microscopy. The scanning electron microscopy results of the HAB / WS2@SiO2 microcapsules are as follows: Figure 1 As shown, the transmission electron microscopy results of HAB / WS2@SiO2 microcapsules are as follows Figure 2 As shown, the optical microscopy results of HAB / WS2@SiO2 microcapsules are as follows Figure 3 As shown. Figures 1 to 3 It can be seen that HAB / WS2@SiO2 microcapsules were successfully prepared, and WS2 was located inside the microcapsule core material instead of on the shell.

[0150] 2. The PAO6 / MoS2@UF microcapsules prepared in Example 2 were observed using a scanning electron microscope. Figure 4 As shown. Figure 4 It can be seen that the particle size is about 1 μm or less.

[0151] 3. The friction coefficient of each lubricating composite material block prepared in Examples 1 to 6 and Comparative Examples 1 to 2 was tested. The specific method is: each lubricating composite material block was tested on a UMT-5 friction and wear tester; the friction coefficient test results of each lubricating composite material block are shown in Table 1. The friction coefficient of the self-lubricating composite material block in Example 1 and Comparative Examples 1 to 2 changes with time as shown in Table 1. Figure 5 shown.

[0152] 5. The lubricating composite material blocks prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were subjected to a use temperature test. The specific method is: liquid nitrogen and a heating chamber are used to control the ambient temperature of the sample; the use temperature results of the lubricating composite material blocks are shown in Table 1.

[0153] 6. The particle size and the mass ratio of the core material to the shell layer of each lubricating microcapsule prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were tested by thermogravimetric analysis (TGA). The test results are shown in Table 1.

[0154] The performance test results of Examples 1 to 6 and Comparative Examples 1 to 2 are shown in Table 1.

[0155] Table 1

[0156]

[0157] From the results of Examples 1 to 6 in Table 1, it can be seen that when the core material contains both liquid lubricant and solid lubricant, the friction coefficient of the prepared lubricating microcapsules can be as low as 0.056, and the use temperature range can be expanded to -50 to 400°C, especially the lowest temperature can reach -50°C; this shows that when the core material contains both liquid lubricant and solid lubricant, the friction coefficient of the lubricating microcapsules can be significantly reduced, while the temperature range of the lubricating microcapsules can be increased.

[0158] The difference between Example 1 and Examples 5-6 is that the ratio of the amount of liquid lubricant and solid lubricant added when preparing the core material is different. The results of Example 1 and Examples 5-6 show that when the ratio of the amount of solid lubricant to liquid lubricant when preparing the core material is 1:(2-100), the friction coefficient of the lubricating microcapsules prepared is smaller and the temperature range is wider.

[0159] The difference between Comparative Examples 1 and 2 and Example 1 is that only a single lubricant is used, and solid lubricants and liquid lubricants are not used simultaneously. Compared with Comparative Examples 1 and 2, the friction coefficient of the lubricating microcapsules in Example 1 is significantly lower than the friction coefficient of the microcapsules in Comparative Examples 1 and 2. The technicians analyzed that the reason is that, compared with Example 1, Comparative Example 1 only has the oil lubrication effect of HAB, without WS2, and cannot produce synergistic lubrication. Comparative Example 2 only has the lubrication effect of WS2, without HAB, and also cannot produce coordinated lubrication.

[0160] At the same time, the use temperature range of the lubricating microcapsules in Example 1 is significantly greater than the use temperature range of the microcapsules in Comparative Examples 1 and 2, and the lowest use temperature in Example 1 is significantly reduced. The technicians analyzed that the reason is that although the liquid lubricant solidifies under low temperature conditions, the solid lubricant is evenly dispersed in the liquid lubricant. When the liquid lubricant solidifies, the solid lubricant can be evenly dispersed on the friction interface, and can still play a good lubricating effect at low temperatures.

[0161] The difference between Comparative Example 3 and Example 1 is that no dispersant is added when preparing the core material in Comparative Example 3. Lubricating microcapsules cannot be prepared in Comparative Example 3, indicating that a dispersant needs to be added to be used together with a solid lubricant and a liquid lubricant when preparing lubricating microcapsules. The dispersant can make the solid lubricant evenly dispersed in the liquid lubricant and prevent the solid lubricant from escaping from the liquid lubricant and entering the water phase, resulting in failure to prepare lubricating microcapsules.

[0162] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0163] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A lubricating microcapsule, characterized in that: include: A core material, wherein the components of the core material include a solid lubricant, a liquid lubricant and a dispersant; the mass ratio of the solid lubricant to the liquid lubricant is 1:(2-100), and the mass of the dispersant accounts for 0.1-10% of the total mass of the solid lubricant and the liquid lubricant; A shell layer, coated on the outside of the core material, wherein the shell layer comprises a shell material, a surfactant and an emulsifier; Wherein, the solid lubricant includes one or more of molybdenum disulfide, tungsten disulfide, graphene, fullerene, black phosphorus, purple phosphorus, magnesium hydroxysilicate, titanium carbide, nano-gold, nano-silver, nano-copper, nano-nickel, nano-iron, nano-zinc, nano-copper oxide, nano-aluminum oxide, nano-zinc oxide and nano-zirconium oxide; the liquid lubricant includes one or more of oil-soluble ionic liquid and lubricating oil; the dispersant includes one or more of Span 80 and boronized polyisobutylene succinimide; The mass ratio of the surfactant to the co-emulsifier is (0.1-5):(0.1-5); the shell material includes one or more of silicon dioxide and urea-formaldehyde resin; the surfactant includes one or more of polyvinyl alcohol, Triton X100, Tween 80, sodium dodecylbenzene sulfonate, ammonium dodecyl sulfate, hexadecyltrimethylammonium bromide, gelatin, gum arabic and lignin; the co-emulsifier includes one or more of n-butanol, ethylene glycol, n-hexadecane, propylene glycol, glycerol and polyglycerol ester.

2. The lubricating microcapsule according to claim 1, characterized in that The lubricating microcapsules meet at least one of the following conditions: (1) The particle size of the lubricating microcapsules is 0.1-100 μm; (2) The mass ratio of the core material to the shell layer in the lubricating microcapsule is (2-4):5; (3) The friction coefficient of the lubricating microcapsules is 0.04 to 0.1; (4) The operating temperature range of the lubricating microcapsules is -50~400°C.

3. The lubricating microcapsule according to claim 1, characterized in that The solid lubricant is one or more of molybdenum disulfide and tungsten disulfide.

4. The lubricating microcapsule according to claim 1, characterized in that The oil-soluble ionic liquid includes one or more of 1-butyl-3-methylimidazolium hexafluorophosphate, 1-octyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-methyl-3-n-octylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-ethyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt and 1-octyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt.

5. The lubricating microcapsule according to claim 4, characterized in that The oil-soluble ionic liquid is 1-butyl-3-methylimidazolium hexafluorophosphate.

6. The lubricating microcapsule according to claim 1, characterized in that The lubricating oil includes one or more of hydrogenated polydecene, linseed oil, alkyl silicone oil, phenyl silicone oil, chain oil, tung oil, mineral oil, ester base oil, liquid paraffin, perfluoropolyether, heavy alkylbenzene and oleic acid.

7. The lubricating microcapsule according to claim 6, characterized in that The lubricating oil is one or more of hydrogenated polydecene, heavy alkylbenzene and phenyl silicone oil.

8. The lubricating microcapsule according to claim 1, characterized in that The surfactant is one or more of polyvinyl alcohol, Triton X100, Tween 80 and gum arabic.

9. The lubricating microcapsule according to claim 1, characterized in that: The auxiliary emulsifier is n-hexadecane.

10. A method for preparing lubricating microcapsules according to any one of claims 1 to 9, characterized in that: The steps include: Mixing the solid lubricant, the liquid lubricant and the dispersant to obtain a core material; Mixing the surfactant, the co-emulsifier and the solvent A to obtain phase A, and adjusting the pH value of phase A; Mixing the shell material precursor and solvent B to obtain phase B; The core material, the phase A and the phase B are mixed and reacted, and the reaction product is dried to obtain the lubricating microcapsules.

11. The method for preparing lubricating microcapsules according to claim 10, characterized in that: When preparing the core material, mechanical stirring or ultrasound is used to mix the solid lubricant, the liquid lubricant and the dispersant.

12. The method for preparing lubricating microcapsules according to claim 11, characterized in that: The mechanical stirring rate is 100~2000rpm, and the mechanical stirring time is 10~20min.

13. The method for preparing lubricating microcapsules according to claim 11, characterized in that: The ultrasonic power is 50~1200W, and the ultrasonic time is 10~120min.

14. The method for preparing lubricating microcapsules according to claim 10, characterized in that: The preparation of the phase A includes at least one of the following conditions: (1) The mass proportion of the surfactant in the phase A is 0.1-5%; (2) The mass proportion of the co-emulsifier in the phase A is 0.1-5%; (3) The pH value of phase A is 2 to 12; (4) The solvent A includes water.

15. The method for preparing lubricating microcapsules according to claim 10, characterized in that: The preparation of the phase B includes at least one of the following conditions: (1) The precursor of the shell material includes tetraethyl orthosilicate or a mixture of urea, formaldehyde and resorcinol or a mixture of tetraethyl orthosilicate, urea, formaldehyde and resorcinol; (2) The mass proportion of the precursor of the shell material in the B phase is 0.2-40%; (3) The solvent B is water or a mixture of ethanol and water.

16. The method for preparing lubricating microcapsules according to any one of claims 10 to 15, characterized in that: The step of mixing the core material, the phase A and the phase B to react specifically comprises: Add the core material into the phase A and disperse it; The phase B is added to the phase A to obtain a mixed solution, and the mixed solution is reacted at 10-100° C. for 30-480 min.

17. The method for preparing lubricating microcapsules according to claim 16, characterized in that: The process used for dispersing the core material and the phase A includes: stirring at a stirring rate of 100-2000 rpm for 5-60 minutes or ultrasonicating at an ultrasonic power of 50-1200 W for 5-60 minutes.

18. The method for preparing lubricating microcapsules according to claim 16, characterized in that: When the phase B is added to the phase A, the phase A is stirred at a stirring rate of 100-2000 rpm or ultrasonicated at an ultrasonic power of 50-1200 W.

19. A self-lubricating composite material, characterized in that: The invention comprises the lubricating microcapsules as claimed in any one of claims 1 to 9 or the lubricating microcapsules prepared by the method as claimed in any one of claims 10 to 18.