A cerium-manganese catalyst for catalytic oxidation of toluene and a preparation method thereof
The cerium-manganese composite catalyst was prepared by hydrothermal synthesis method, and the rod-like structure was formed by controlling the concentration of alkali liquid and the hydrothermal temperature, which solved the problem of insufficient catalyst activity, significantly improved the low-temperature catalytic oxidation performance, catalytic activity and crystals of cerium oxide and manganese oxide. The surface compound is closely related to achieve efficient catalytic toluene.
Patent Information
- Application Number
- CN202310167983.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The existing catalysts are insufficiently active during the catalytic oxidation process of toluene, which is difficult to effectively catalyze under low temperature conditions, and the synergistic effect of the active crystal surface in the multi-component catalyst is not fully utilized.
The cerium-manganese composite catalyst was prepared by hydrothermal synthesis method, and the rod-like structure of cerium oxide was controlled by alkali liquid concentration and hydrothermal temperature, which strengthened the formation of active crystal surfaces and improved the low-temperature catalytic oxidation performance of the catalyst.
The low-temperature catalytic oxidation performance of the catalyst is significantly improved, and the catalytic activity improvement is closely related to the recombination of the active crystal surfaces (200), (111) and the (222) of manganese oxide, forming the Mn-Ce composite of rod-like structure Catalysts can catalyze toluene efficiently at low temperatures.
Smart Images

Figure CN116251585B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation and catalytic oxidation of environmental pollutants, and relates to a cerium manganese catalyst for catalytic oxidation of toluene and a preparation method thereof. Background Art
[0002] VOCs from industrial sources have the characteristics of large emissions, many types, and high toxicity, which has become a difficult problem for environmental governance. People have developed a variety of governance strategies based on the characteristics of waste gas in the environment, such as absorption, adsorption, oxidation, and biodegradation. Among them, the catalytic oxidation method uses the deep redox ability of the catalyst to combine the organic components with oxygen at a temperature below the ignition point of 250 to 400 ° C to generate non-toxic products. This method has many advantages such as low reaction starting temperature, low energy consumption, high efficiency and no secondary pollution, and has attracted widespread attention. Catalysts for the catalytic oxidation of VOCs include precious metals and non-precious metal catalysts. Due to the cost of raw materials and resource limitations, people will choose more easily available non-precious metal oxides as catalysts for treating VOCs.
[0003] In recent years, many studies have shown that the activity of catalysts is closely related to the morphology and crystal surface of their materials.
[0004] Ren et al. synthesized Co3O4 nanocatalysts with different morphologies and exposed crystal faces by hydrothermal method, including microspheres ({111}), flower-shaped ({110}), sea urchin-shaped ({110}) and fan-shaped ({112}), and applied them to the catalytic oxidation of toluene. The results of their catalytic evaluation confirmed that the activity of different exposed crystal faces follows the order of {110}>{111}>{112}.
[0005] Quan et al. prepared aerogel (CeO2-A), nanorods (CeO2-R) and nanosheets (CeO2-F) cerium oxide materials by different synthesis methods. Among them, aerogel cerium oxide (CeO2-A) with exposed (100) and (111) crystal planes has excellent catalytic activity for the oxidation of toluene. 90 =239℃.
[0006] When Zhang Zhaoliang et al. studied NO oxidation, they found that rod-shaped Mn2O3 materials with exposed (222) crystal planes had significant resistance to H2O poisoning.
[0007] When studying the selective growth of cerium oxide materials, Mai et al. found that isotropic materials, when grown without templates, usually obtain spherical particles. Cerium oxide is an isotropic structural material and it is difficult to grow anisotropically under the same conditions. However, when the alkali concentration in the solution is high (C NaOH>1M), the Ce(OH)3 intermediate can continue to grow into nanorod-like crystals due to the significant increase in the dissolution / recrystallization rate. At the same time, the intermediate species is not stable and tends to form cubic particles when the hydrothermal temperature is greater than 180°C.
[0008] In addition, Cheng found that the activity of the catalyst under isothermal conditions depends on the size of the exposed crystal surface area rather than the specific surface area of the material.
[0009] In summary, in the process of catalyst preparation, optimizing the growth of active crystal faces, giving full play to the role of the active crystal faces of each component, and exploring the synergistic effect of multiple active crystal faces in multi-component catalysts are of vital importance to obtaining catalysts with excellent performance. Summary of the invention
[0010] Technical problem to be solved: By exposing the active crystal faces of each component in the Mn-Ce composite oxide and exerting a synergistic effect, the catalytic oxidation activity of the catalyst for toluene is improved. The cerium-manganese composite catalyst prepared by the present invention is prepared by a hydrothermal synthesis method, and the purpose is to strengthen the formation of active crystal faces during the catalyst preparation process to improve the low-temperature catalytic oxidation performance of toluene in the catalyst.
[0011] Technical solution: Using Ce without template 3+ The species forms an "intermediate", which is a necessary condition for the anisotropic growth of the catalyst in the solution. The rod-shaped structure of cerium oxide is formed by controlling the concentration of the alkali solution and the hydrothermal temperature. Since the reactor is operated under high pressure, the hydrothermal reaction is carried out at a temperature higher than the boiling point, which can intensify ion collision and adsorption. Since the particle size of cerium oxide particles is larger than that of manganese oxide, the manganese oxide particles will be deposited, adsorbed or agglomerated on the surface or around the rod-shaped cerium oxide.
[0012] Furthermore, the soluble cerium salt is any one of Ce(SO4)3, CeCl3, and Ce(NO3)3·6H2O, preferably Ce(NO3)3·6H2O.
[0013] Furthermore, the soluble manganese salt is any one of MnCl2, Mn(CH3COO)2, and Mn(NO3)2·4H2O, preferably Mn(NO3)2·4H2O.
[0014] Furthermore, the precipitant is any one of KOH, NaOH, and NH3·H2O.
[0015] Furthermore, the concentration of the alkali solution is 2 to 10 moL / L.
[0016] Furthermore, the water temperature is controlled at 100-200°C.
[0017] Furthermore, the active crystal planes (100) and (111) of cerium oxide are exposed, and the dominant crystal plane (222) of manganese trioxide is exposed.
[0018] Furthermore, the catalyst is applied to various VOCs-polluted exhaust gases.
[0019] Beneficial effects of the present invention:
[0020] 1. During hydrothermal synthesis, the rod-shaped Mn-Ce composite catalyst is prepared by controlling the temperature and alkali solution concentration.
[0021] 2. The improvement of catalytic activity is not only due to its specific surface area, but also closely related to the active crystal faces (200) and (111) of cerium oxide and its complex with the crystal face (222) of manganese oxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 (a) is the XPS spectrum of catalyst #2; (b) is the XPS spectrum of catalyst #3.
[0023] Figure 2 (a, d) are spherical catalyst #1; (b, e) are spherical catalyst #2;
[0024] (c, f) are TEM images of rod-shaped catalyst #3.
[0025] Figure 3 XRD patterns of catalysts 2# and 3#.
[0026] Figure 4 This is the performance diagram of catalytic oxidation of toluene by catalyst samples 1#, 2#, and 3#. DETAILED DESCRIPTION
[0027] In the following examples, the catalytic oxidation performance of toluene was evaluated in the following manner: (1) Catalyst pretreatment: The catalyst for catalytic oxidation was first sieved through 40-60 mesh for standby use, and 0.5g of the treated catalyst was mixed with 1.5g of quartz sand and loaded into a fixed bed reaction tube (id=17mm); (2) Catalytic oxidation reaction of toluene: The catalytic performance was determined in a fixed bed stainless steel reaction tube. Specific process: Before the reaction, nitrogen was introduced at a flow rate of 100mL / min to blow away impurities in the gas path; then a toluene mixed gas was introduced at a flow rate of 20mL / min, and continuous catalytic oxidation of toluene was performed in a temperature range of 60-300°C. The toluene mixed gas was 1500ppm toluene under a zero-degree water bath, and the air velocity was 14400mL / (g·h). The toluene inlet and outlet concentrations were determined by a gas chromatograph.
[0028] At different temperatures, toluene conversion rate (X toluene ) is calculated according to the following formula:
[0029] Xtoluene =[(C toluene,n )-(C toluene,nt ) / C toluene,n ]×100%
[0030] Among them, C toluene,n is the inlet toluene concentration, C toluene,nt is the outlet toluene concentration (ppm).
[0031] Example 1
[0032] Preparation of Mn2O3 catalyst
[0033] (1) 4 mmol of 50% Mn(NO3)2·4H2O was dissolved in 20 mL of deionized water and stirred to fully dissolve. Then, 60 mL of 2 mol / L NaOH solution was added dropwise and stirred vigorously for 30 min.
[0034] (2) The mixed suspension was transferred to a Teflon reactor and the hydrothermal temperature was maintained at 100°C for 24 hours. The precipitate after the reaction was filtered and washed with deionized water first and then with anhydrous ethanol.
[0035] (3) The obtained solid was dried at 60°C for 12 hours. In an air atmosphere, the temperature was raised to 500°C at a heating rate of 2°C / min and calcined at the constant temperature for 2 hours. The prepared Mn2O3 metal oxide was recorded as "1#".
[0036] Example 2
[0037] Ce1Mn2O x Preparation of -100℃ catalyst
[0038] (1) Weigh 4 mmol Ce(NO3)3·6H2O and 8 mmol Mn(NO3)2·4H2O (50% by mass) and dissolve them in deionized water. Stir until they are fully dissolved. Then, add 60 mL of 2 mol / L NaOH solution dropwise and stir vigorously for 30 min.
[0039] (2) The mixed suspension was transferred to a Teflon reactor and the hydrothermal temperature was maintained at 100°C for 24 hours. The precipitate after the reaction was filtered and washed with deionized water first and then with anhydrous ethanol.
[0040] (3) The obtained solid was dried at 60°C. In an air atmosphere, the temperature was raised to 500°C at a heating rate of 2°C / min and calcined at this temperature for 2 h. x -100℃ metal oxide, recorded as "2#".
[0041] Example 3
[0042] Ce1Mn2Ox Preparation of -150℃ Catalyst
[0043] (1) Weigh 4 mmol Ce(NO3)3·6H2O and 8 mmol 50% Mn(NO3)2·4H2O solution, stir to fully dissolve. Then, drop 60 mL 2 mol / L NaOH solution and stir vigorously for 30 min.
[0044] (2) The mixed suspension was transferred to a Teflon reactor and the hydrothermal temperature was maintained at 150°C for 24 hours. The precipitate after the reaction was filtered and washed with deionized water first and then with anhydrous ethanol.
[0045] (3) The obtained solid was dried at 60°C for 12 h. In an air atmosphere, the temperature was raised to 500°C at a heating rate of 2°C / min and calcined at this temperature for 2 h. x -150℃ metal oxide, marked as "3#".
[0046] (1) Chemical composition analysis
[0047] Table 1 XPS element content of catalysts 2# and 3#
[0048]
[0049] According to the research results of Mai et al., low temperature (<180℃) and high alkali concentration (C NaOH >1M) can promote the anisotropic growth of the intermediate Ce(OH)3 into rod-shaped crystals.
[0050] Depend on Figure 1 (a) From the XPS spectrum of catalyst #2, it can be seen that the peaks with binding energies of 885.8 eV (V1) and 904.3 eV (U1) are Ce. 3+ Characteristic peaks, the remaining V, V2, V3, U, U2, U3 peaks are Ce 4+ Characteristic peaks. According to the peak area calculation of the XPS spectrum, the information in Table 1 is obtained. It can be seen that when other preparation conditions are the same, as the hydrothermal reaction temperature increases from 100℃ to 150℃, the Ce of catalysts 2# and 3# increases. 3+ / (Ce 3+ +Ce 4+ ) relative content increased from 11.22% to 24.48%, which may be due to the fact that the experimental conditions are prone to the formation of the intermediate Ce(OH)3 or the transfer of valence electrons between manganese and cerium elements. Figure 1XPS analysis of (a, b) shows that both catalysts 2# and 3# contain +3 and +4 manganese elements, MnO2 and Mn2O3 exist on the surface of the samples, and the +3 manganese content is higher than the +4 manganese content. The samples may contain most of Mn2O3 and less MnO2.
[0051] In order to determine the morphological changes of the catalysts of Example 2 and Example 3, TEM analysis was performed on the samples. Figure 2 (b) and (c) show that catalyst #2 is spherical while catalyst #3 is rod-shaped. The increase in the hydrothermal reaction temperature may reduce the formation of intermediate content, thereby changing the tendency of anisotropic growth.
[0052] (2) Crystal plane and morphology analysis
[0053] In order to confirm the morphology and exposed crystal surface information of Example 1, Example 2 and Example 3, TEM and XRD analyses were performed on the samples.
[0054] like Figure 2 (d), (e) and (f) are the high-resolution images of samples 1#, 2# and 3#, respectively. Figure 2 (d) indicates that the (222) crystal plane of sample 1 Mn2O3 has a crystal plane spacing d(hkl) of 0.27 nm; Figure 2 (e) and (f) respectively represent the d(hkl)=0.31nm CeO2(111), d(hkl)=0.27nm CeO2(200) crystal plane and Mn2O3(222) crystal plane of samples 2# and 3# Mn2O3@CeO2.
[0055] XRD analysis of the samples, such as Figure 3 As shown. The diffraction peaks at 2θ=29°, 48°, and 57° of the sample correspond to the (111), (220), and (311) crystal planes of CeO2 (PDF#43-1002). Among them, the peak intensity of the diffraction peak at 2θ=34° corresponding to the (200) crystal plane of CeO2 is relatively small, indicating that the surface CeO2 (200) crystal planes in the components of sample 2# and sample 3# are less exposed, while the surface of the sample mainly exposes more CeO2 (111) crystal planes. The diffraction peak at 2θ=33° of the sample corresponds to the (222) crystal plane of bixbyite Mn2O3 (PDF#41-1442). From the diffraction peak at 2θ=33°, it can be seen that the peak intensity of sample 3# is significantly greater than that of sample 2# and is sharper. This indicates that in the composite catalyst, the surface Mn2O3 (222) crystal plane of sample 3# is more exposed than that of sample 2# and has better crystallinity.
[0056] Since the surface energy of CeO2(200) crystal plane is lower than that of CeO2(111) crystal plane, when the hydrothermal temperature increases, the growth of crystals tends to expose low-index crystal planes to reduce chemical potential. Therefore, CeO2(111) crystal plane exposure should be less. This is inconsistent with the XRD analysis. In order to explore the specific reasons, TEM analysis was performed on samples 2# and 3#. Figure 2 (f) It is found that the rod-shaped CeO2 has a low surface energy CeO2 (200) crystal plane, but the surface is also distributed with CeO2 (111) crystal plane and Mn2O3 (222) crystal plane. The results show that the surface of the rod-shaped CeO2 is covered with spherical Mn2O3 and CeO2 particles, which hinders the exposure of the CeO2 (200) crystal plane. The high-index CeO2 (111) crystal plane is considered to be the most active crystal plane.
[0057] The exposure of more CeO2(111) crystal faces may be one of the reasons for the good catalyst activity.
[0058] In order to evaluate the activity of the exposed crystal faces of samples 1#, 2#, and 3#, toluene was used as a representative volatile organic pollutant for testing. The activity results are shown in Figure 4 As shown in the figure, the toluene degradation rates of samples 1#, 2#, and 3# are t 90 =280℃、t 90 =250℃ and t 90 =230℃. The results show that the composite components of samples 2# and 3# have better catalytic effects than the single component sample 1#. The difference in activity between samples 2# and 3# may be due to the combination of manganese and cerium components, that is, the spherical clusters and rod-shaped morphologies of manganese and cerium oxides, which leads to different numbers of exposed crystal faces CeO2(200) and Mn2O3(222) on the sample surface.
[0059] (3) Specific surface area and activity analysis
[0060] Table 2 BET specific surface area, pore volume and pore diameter parameters of catalysts 1#, 2# and 3#
[0061]
[0062] In order to confirm the relationship between the specific surface area and activity of the materials of samples 1#, 2#, and 3#, the BET test was performed on the samples, as shown in Table 2. The surface area of samples 1#, 2#, and 3# is 20.717 m 2 / g, 67.946m 2 / g, 44.037m 2 / g. The order of specific surface area of the samples is 2#>3#>1#, while the order of activity among the samples is 3#>2#>1#. The results show that the specific surface area of the sample is not the decisive factor for activity. As Cheng et al. confirmed, the activity of the catalyst under isothermal conditions depends on the size of the exposed crystal surface area, rather than the specific surface area of the material.
[0063] From the above examples, we can see that the activity of the catalyst is not only related to its specific surface area and its chemical composition, but also to the catalyst morphology, the type and abundance of exposed crystal faces. Therefore, appropriate hydrothermal reaction temperature adjustment is conducive to the formation of anisotropic intermediates, which facilitates the catalyst to form a favorable rod-like morphology and improves its catalytic oxidation activity for VOCs.
[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a cerium manganese catalyst for catalytic oxidation of toluene, characterized in that: Using soluble cerium salt and manganese salt as raw materials and alkali as precipitant, under hydrothermal conditions, adjusting the hydrothermal temperature and appropriate alkali solution concentration to react, a cerium-manganese composite catalyst with a rod-like morphology and exposed active crystal faces and dominant crystal faces is obtained; The soluble cerium salt is Ce(NO3)3·6H2O; The soluble manganese salt is Mn(NO3)2·4H2O; The precipitant is NaOH with a concentration of 2moL / L; The hydrothermal temperature was controlled at 150°C; The preparation method is: (1) Weigh 4 mmol Ce(NO3)3·6H2O and 8 mmol 50% Mn(NO3)2·4H2O solution, stir to fully dissolve, then drop 60 mL 2 mol / L NaOH solution and stir vigorously for 30 min. (2) The mixed suspension was transferred to a Teflon reactor and the hydrothermal temperature was maintained at 150° C. for 24 h. The precipitate after the reaction was filtered and washed with deionized water and then with anhydrous ethanol; (3) The obtained solid was dried at 60°C for 12 h, heated to 500°C at a heating rate of 2°C / min in an air atmosphere, and calcined at a constant temperature for 2 h to prepare Ce1Mn2O x -150℃ metal oxides.
2. A cerium-manganese catalyst for catalytic oxidation of toluene, characterized in that: The method according to claim 1 is used to prepare the