A heavy oil type in-situ crystallization catalyst and preparation method thereof

By introducing silicon-aluminum materials with a supra-thin hydrolaminite structure into the in situ crystallization catalyst, the problem of insufficient pore volume and specific surface area of ​​the existing catalyst is solved, the heavy oil conversion capacity and environmental friendliness are improved, and the heavy oil catalysis is achieved efficient Effect.

CN116251615BActive Publication Date: 2024-11-05PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111502789.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-09
Publication Date
2024-11-05
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

The existing in-situ crystallization catalysts have insufficient pore volume and specific surface area in heavy oil conversion, resulting in weak conversion capacity of heavy oil and environmental pollution problems, such as carbon emissions and air pollution caused by high-temperature roasting.

Method used

Using silicon-aluminum material with a phthalinite structure, the silicon-aluminum material with a phthalinite structure is formed into glue through a co-flow of acidic aluminum sources and alkaline aluminum sources, and the silicon source is added online, and multiple exchanges and calcination are performed to prepare a 2-40nm and 70- A high pore volume catalyst with a bipolar distribution of 300nm.

Benefits of technology

The pore volume and specific surface area of ​​the catalyst are improved, the heavy oil conversion capacity and gasoline yield are enhanced, environmental pollution is reduced, and the catalyst has higher thermal stability and acid amount.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116251615B_ABST
    Figure CN116251615B_ABST
Patent Text Reader

Abstract

The present invention relates to a heavy oil type in-situ crystallization catalyst. The raw material of kaolin microspheres for preparing the catalyst contains a silicon aluminum material. The silicon aluminum material has a pseudo-boehmite structure. The anhydrous chemical expression thereof is (0-0.2) Na2O: (4-30) SiO2: (70-96) Al2O3, based on the weight of the oxide. The silicon aluminum material has a double pore distribution of 2-40 nm and 70-300 nm, and a specific surface area of ​​more than 500 and not more than 650 m 2 / g, the pore volume is 2.1-2.8ml / g, and the ratio of the pyridine infrared B acid amount to the L acid amount measured at 200°C is 0.10-0.38. The present invention introduces a silicon-aluminum material with a higher pore volume, a larger specific surface area, a B acid center and a double pore distribution into the catalyst to prepare an in-situ crystallization type catalytic cracking catalyst with strong heavy oil conversion ability and high gasoline yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil refining catalysts, and in particular relates to a heavy oil type in-situ crystallization catalyst and a preparation method thereof. Background Art

[0002] my country's dependence on foreign crude oil has reached 73%. Maximizing the utilization of crude oil is an important challenge facing crude oil processing. In recent years, the proportion of high-sulfur heavy crude oil in domestic imported crude oil has gradually increased. At the same time, the quality of domestic crude oil is poor, and the trend of heavy and inferior crude oil processed by domestic refineries is obvious. Heavy oil catalytic cracking is an important means of heavy oil processing in my country, accounting for about 38% of the primary processing capacity. Optimizing the catalyst is the most economical, effective and rapid means to improve the conversion capacity of catalytic cracking heavy oil.

[0003] Catalytic cracking catalysts are divided into two categories: semi-synthetic catalysts and in-situ crystallization catalysts. Due to its special preparation route, in-situ crystallization catalysts have the characteristics of developed pore structure and strong resistance to heavy metals, and play an important role in the conversion of catalytic cracking heavy oil. However, due to the process characteristics of preparing microspheres first and then forming molecular sieves and matrices simultaneously through in-situ crystallization technology, its composition and structure cannot be adjusted as flexibly as semi-synthetic catalysts. The introduction of new processes, new methods and new materials is an important way to improve the conversion of heavy oil by in-situ crystallization catalysts.

[0004] CN1778676A proposes a method for preparing a high-content NaY molecular sieve by synthesizing kaolin spray microspheres, wherein one or more of starch, graphite powder, and carboxymethyl cellulose are added as structural additives to the spray soil balls to improve the structure of the soil balls, and a high-content NaY molecular sieve is obtained after crystallization. However, the structural additives need to be removed by roasting, which increases the carbon emissions in the catalyst production.

[0005] The in-situ crystallization catalyst synthesized in USP 4493902, 6656347, 6696378, 6942783, 6943132, and CN 01817891.X has macropores of 60nm to 2000nm, but this technology has very high requirements for the raw materials used for spray molding. In order to stack more macropores, the importance of ultra-fine original soil and ultra-fine high soil is emphasized, but this soil is expensive and difficult to buy on the market. At the same time, the catalyst synthesized by this method has low strength. In order to increase the strength of the catalyst, silicon retention technology needs to be further adopted for the crystallized product.

[0006] CN201210061876.8 discloses a method for preparing a catalytic cracking promoter, which introduces a compound with a boiling point of 150°C or less or a compound that decomposes and completely converts into gas at 150°C into a kaolin spray slurry, and introduces rich mesopores and macropores into an in-situ crystallization catalyst. However, the compound is easy to enter the atmosphere during the spray drying process, causing air pollution.

[0007] CN201010262279.2 provides a method for preparing NaY zeolite, which introduces polydimethyldiallyl ammonium chloride into kaolin microspheres to improve the pore structure of the microspheres, thereby obtaining a high-crystallinity crystallized product. However, high-temperature calcination and removal of polydimethyldiallyl ammonium chloride also poses an environmental pollution problem.

[0008] CN110523429A provides a method for preparing an in-situ crystallized catalytic cracking catalyst, wherein calcined kaolin microspheres are pretreated with alkali solution, and then a guiding agent is added for crystallization. After the crystallization is completed, the corresponding in-situ crystallized catalyst is obtained through exchange and calcination steps. The prepared catalyst has the characteristics of large pore volume and low bulk ratio. However, the pretreatment step of the microspheres in the invention is likely to affect the wear index of the catalyst.

[0009] Alumina materials are important catalytic carrier materials and are also widely used in catalytic cracking catalysts. They are active carrier materials for semi-synthetic catalytic cracking catalysts. Alumina materials can also be used in in-situ crystallization catalysts. CN200480014012.4 provides an FCC catalyst prepared by in-situ crystallization of zeolite. The catalyst is a fluid catalytic cracking catalyst with high porosity, which is provided by in-situ crystallization of aluminosilicate zeolite from reactive microspheres containing metakaolin and hydrous kaolin. The application document also discloses the preparation of metal-resistant alumina microspheres. The reaction performance of the in-situ crystallization catalyst can be adjusted by introducing metal-resistant calcined boehmite into the microspheres.

[0010] Alumina is used as a catalyst carrier for catalytic cracking. Its pore structure and acidic properties affect the reaction performance of the catalyst. In order to improve the reaction performance of the catalyst, a large number of studies have been devoted to modifying alumina, preparing macroporous alumina, or preparing macroporous silicon-alumina materials to replace the existing alumina carrier.

[0011] Zheng Jinyu et al. (Petroleum Refining and Chemical Engineering, 2015, 46(9): 47-51) successfully prepared a disordered mesoporous silica-alumina material (JSA) with a pseudo-boehmite structure through gelation and aging processes. The material has a high specific surface area and pore volume, with a specific surface area of ​​300m 2 / g or more, pore volume greater than 0.7cm 3 / g, and the pore size is between 6 and 7 nm.

[0012] Maryam Khosravi Mardkhe (Applied Catalysis, A: General, 2014, 482: 16-23.) et al. introduced a silicon-doped alumina material. XRD showed that it still had the characteristic diffraction peaks of alumina. By adjusting the silicon content, large pore volume and large pore diameter silicon-doped alumina can be obtained, with a pore volume of 0.33 to 1.83 cm 3 / g range, the maximum pore size can reach 51.6nm.

[0013] CN03147975.8 introduces a mesoporous silicon-aluminum material with a pseudo-boehmite phase structure. The anhydrous chemical expression based on the weight of the oxide is: (0-0.3)Na2O·(40-90)Al2O3·(10-60)SiO2, and its specific surface area is 200-400m 2 / g, the pore volume is 0.5~2.0mL / g, the average pore diameter is 8~20nm, and the most probable pore diameter is 5~15nm.

[0014] CN201110251792.6 The invention provides an acidic silicon-aluminum catalytic material having a pseudo-boehmite crystal phase structure; its anhydrous chemical expression, measured by oxide weight, is: (0-0.2)Na2O·(44-46)SiO2·(54-56)Al2O3, the pore volume is 0.5-1.0mL / g, and the average pore diameter is 8-15nm.

[0015] The invention of CN201110251761.0 provides a mesoporous acidic silicon-aluminum catalytic material having a pseudo-boehmite crystal phase structure. Its anhydrous chemical expression is (0-0.2)Na2O·(16-20)SiO2·(80-84)Al2O3, based on the weight of the oxide, with a pore volume of 1.0-2.0mL / g and an average pore diameter of 8-20nm. The ratio of pyridine infrared B acid to L acid measured at 200°C of the material is 0.060-0.085.

[0016] CN201210409663.X provides a method for preparing silicon-containing alumina dry glue. The prepared silicon-containing alumina dry glue is calcined at 500°C to 950°C for 2 to 6 hours. The properties of the obtained silicon-containing alumina are as follows: the pore volume is 0.55 to 1.10 mL / g, and the pore volume of pores with a pore diameter of 10 nm to 50 nm accounts for 30% to 80% of the total pore volume.

[0017] Xu benjing et al. (Microporous and Mesoporous materials 238 (2017): 84-89) introduced water glass as a silicon source into the alumina synthesis system to synthesize silicon-containing alumina materials, and investigated the effects of 3%, 6%, 12% and 24% silicon oxide addition on the pore structure of the product. The pore volume of the synthesized material reached up to 1.46 cm 3 / g, with a specific surface area of ​​427m 2 / g.

[0018] CN201510861407.8 introduces an active mesoporous silicon-aluminum catalytic material having a pseudo-boehmite crystal phase structure and a specific surface area of ​​200 to 600 m 2 / g, the pore volume is 0.5-2.0mL / g, the average pore diameter is 8-20nm, and the ratio of the pyridine infrared B acid content to the L acid content measured at 200°C is 0.055-0.085.

[0019] CN201510864343.7 provides a method for preparing an active catalytic material, which has a pseudo-boehmite crystal phase structure, and its anhydrous chemical expression is (0-0.2)Na2O·(10-60)SiO2·(40-90)Al2O3, based on the weight of the oxide, and its specific surface area is 200-600m 2 / g, pore volume of 0.5-2.0ml / g, average pore size of 8-20nm, particle size distribution of the catalytic material is D(V,0.5)≤4μm, D(V,0.9)≤12μm, and the ratio of pyridine infrared B acid to L acid measured at 200°C is 0.055-0.085. The invention obtains better pore volume and smaller material particle size by online addition of silicon source. The preparation method of the material comprises the following steps: (1) neutralizing an aluminum source and an alkaline solution sodium metaaluminate at room temperature to 85°C to form a gel, and controlling the pH value of the gel process to be maintained at 7-11; (2) adding the required silicon source to the gel slurry in a parallel flow manner in the neutralization gel process according to the weight ratio of SiO2:Al2O3=1:(0.6-9) to achieve online addition of the silicon source, and then aging at room temperature to 90°C for 1-10 hours; (3) exchanging the obtained solid precipitate at room temperature to 100°C for 1-3 times according to the weight ratio of solid precipitate (dry basis): ammonium salt: H2O=1:(0.1-1):(10-30), each time for 0.5-1 hour, until the sodium content in the solid precipitate is less than 0.2%. The active catalytic material obtained by the method provided by the present invention has obvious mesopore characteristics, smaller particle size, contains B acid and L acid centers, and the ratio of B acid to L acid is high, and the material has higher cracking activity.

[0020] CN201710382520.7 discloses a porous catalytic material, the XRD spectrum of which shows a diffuse diffraction peak at a 2θ angle of 25° to 27°, and a FAU crystal phase structure exists at the same time, and its chemical composition contains 50 to 80% silicon and 20 to 50% aluminum by weight of oxide, the total specific surface area is ≯250m2 / g, the ratio of micropore specific surface area to total specific surface area is ≯28%, and the ratio of the number of B acid centers to the number of L acid centers measured by pyridine infrared at 200°C is ≥0.30; when the surface Al / Si atomic ratio measured by XPS method is a, and the bulk Al / Si atomic ratio measured by XRF method is b, a / b=1.1 to 1.6. The material is a mixture of amorphous silicon aluminum oxide and zeolite.

[0021] CN201710382478.9 discloses a highly active catalytic material, wherein the XRD spectrum of the catalytic material has characteristic diffraction peaks of pseudo-boehmite structure at 2θ angles of 14°, 28°, 38.5°, 49° and 65°, the ratio of the number of B acid centers to the number of L acid centers measured by pyridine infrared at 200°C is 0.10-0.23, the chemical composition calculated by weight of oxides contains 15-45% silicon and 55-85% aluminum, and the specific surface area is 300-500m 2 / g, the average pore size is 5-18nm, when c is the surface Al / Si atomic ratio measured by XPS method, d is the bulk Al / Si atomic ratio measured by XRF method, c / d=1.2-1.6. The preparation method of the material is: adding a silicon source and an alkaline aluminum source into a container in a parallel flow manner at room temperature to 60°C and stirring, controlling the pH value to be 13-14 to mix and form a gel, then adding an acidic aluminum source, and controlling the end point pH value of the slurry system to be 8.0-10.5, then treating at a constant temperature of 40-80°C, washing, filtering, and ion exchange of the obtained solid precipitate to remove impurity ions, wherein the weight ratio of the silicon source to the aluminum source is 1:(1.2-5.7), the silicon source is calculated as silicon oxide, the aluminum source is calculated as aluminum oxide, and is the sum of the alkaline aluminum source and the acidic aluminum source.

[0022] At present, although there have been many reports on the preparation of silicon-containing alumina, silicon-containing alumina precursors, or silicon-alumina materials, the pore volume of the materials is generally less than 2.0 ml / g, and the specific surface area is generally 500 m 2 g -1 Below, and the pore size is small, and it is mainly a single pore distribution. For macromolecular cracking, such as catalytic cracking, due to the wide distribution of heavy oil molecular size, the material is often required to have a double pore or multi-level pore distribution. Summary of the invention

[0023] Based on the above, the main purpose of the present invention is to provide a heavy oil type in-situ crystallization catalyst, by introducing a silicon-aluminum material with a higher pore volume, a larger specific surface area, containing B acid centers and having a double pore distribution into an in-situ crystallization type catalytic cracking catalyst, to prepare an in-situ crystallization type catalytic cracking catalyst with strong heavy oil conversion ability and high gasoline yield.

[0024] To this end, the present invention provides a heavy oil type in-situ crystallization catalyst. The kaolin microsphere raw material for preparing the catalyst contains a silicon aluminum material. The silicon aluminum material has a pseudo-boehmite structure. Its anhydrous chemical expression is (0-0.2) Na2O: (4-30) SiO2: (70-96) Al2O3, based on the weight of the oxide. It has a double pore distribution of 2-40nm and 70-300nm, and a specific surface area of ​​more than 500 and not more than 650m 2 / g, the pore volume is 2.1-2.8ml / g, and the ratio of the pyridine infrared B acid content to the L acid content measured at 200°C is 0.10-0.38.

[0025] The heavy oil type in-situ crystallization catalyst of the present invention is preferably that the amount of silicon-aluminum material added to the kaolin microsphere raw material is 1-10% of the mass of kaolin; more preferably 2-8%.

[0026] The heavy oil type in-situ crystallization catalyst of the present invention is preferably prepared by the following steps:

[0027] (1) preheating the acidic aluminum source and sodium aluminate solution to 45-70° C. respectively, adding them into the reaction kettle in parallel, maintaining the temperature at 45-70° C., stirring the reaction, and the pH value of the reaction is 6-8;

[0028] (2) adding a silicon source at a weight ratio of SiO2:Al2O3=0.05-0.43:1, and adding an alcohol solvent and stirring evenly for primary aging, maintaining the primary aging temperature at 45-70°C and the primary aging pH value at 6-8;

[0029] (3) heating to 80-100° C., adding an alkaline solution to adjust the pH value to 8.5-10.0, and performing secondary aging under stirring to obtain a solid precipitate;

[0030] (4) Filter, wash, exchange and dry the obtained solid precipitate.

[0031] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst described in the present invention, the preheating first heats the acidic aluminum source and sodium aluminate reaction materials to a certain temperature, which can be achieved in various ways, such as water bath heating, steam heating, and oil bath heating.

[0032] In the preparation method of the silicon-aluminum material of the heavy oil type in-situ crystallization catalyst of the present invention, the filtering, washing, exchanging and drying of the obtained solid precipitate are conventional technical means in the art, and the exchanging refers to the ammonium exchange and / or acid exchange at 60-100° C. after the product is washed. The following process conditions are recommended for the ammonium exchange: the solid precipitate is exchanged at 60-100° C. according to the weight ratio of precipitate (dry basis): ammonium salt: H2O=1:(0.1-1):(5-10); exchange 1-3 times, each exchange for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.2wt%. The ammonium salt used for the exchange is selected from one or more of ammonium chloride, ammonium nitrate, ammonium carbonate, ammonium sulfate and ammonium bicarbonate. The acid exchange is recommended to use the following process conditions: the solid precipitate is mixed in a weight ratio of precipitate (dry basis): H2O=1:(5-10), then the pH is adjusted to 2.5-3.5 with an acid solution, and the exchange is carried out at 60-100°C; the exchange is performed 1-3 times, each time for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.3wt%. The acid solution used for the exchange is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and citric acid solutions.

[0033] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, the drying is a general technology and can be carried out in an oven, or by spray drying or flash drying.

[0034] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, the acidic aluminum source is one or more of aluminum nitrate, aluminum sulfate and aluminum chloride.

[0035] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, the concentration of the acidic aluminum source is 50-150 g / L in terms of alumina, and the concentration of the sodium aluminate solution is 20-130 g / L in terms of alumina.

[0036] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, the silicon source is selected from one or more of water glass, sodium silicate and silicate compounds.

[0037] In the preparation method of the silicon-aluminum material of the heavy oil-based in-situ crystallization catalyst of the present invention, it is preferred that in step (2), the silicon source and the alcohol solvent are added simultaneously, or the silicon source is added first and then the alcohol solvent.

[0038] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, the acidic aluminum source is calculated by weight of aluminum oxide, and the amount of the alcohol solvent added is 1-10 times, preferably 2-5 times, the acidic aluminum source.

[0039] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, the alcohol solvent is a compound in which hydrogen atoms in saturated aliphatic hydrocarbons and / or alicyclic hydrocarbons are replaced by hydroxyl groups.

[0040] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst described in the present invention, the alcohol solvent is a C1-C8 monohydric alcohol, dihydric alcohol or trihydric alcohol, preferably a C2-C4 alcohol, and further preferably, the alcohol solvent is selected from one or more of ethanol, ethylene glycol, propanol, glycerol, butanol and butanediol.

[0041] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, the first aging time is 0.5-3h, and the second aging time is 0.5-3h.

[0042] In the preparation method of the silicon-aluminum material of the heavy oil-type in-situ crystallization catalyst of the present invention, it is preferred that the alkaline solution is selected from one or more of ammonia water, sodium aluminate solution, water glass, and sodium hydroxide solution.

[0043] To this end, the present invention also provides a method for preparing a heavy oil-based in-situ crystallization catalyst, comprising the following steps:

[0044] (1) Preparation of in-situ crystallization products by kaolin microspheres

[0045] Kaolin is used as raw material, deionized water and silicon-aluminum materials are added, and the prepared mixed slurry is spray-dried to obtain kaolin spray microspheres, which are then roasted, mixed with silicon source, alkaline solution and directing agent for crystallization, and the filter cake is filtered, washed and dried to obtain an in-situ crystallization product; the amount of silicon-aluminum materials added is 1-10% of the mass of kaolin, preferably 2-8%;

[0046] (2) The in-situ crystallization product is subjected to exchange and calcination to prepare an in-situ crystallization catalyst

[0047] The in-situ crystallization product is exchanged and calcined with one or more of ammonium salt, rare earth or phosphorus to obtain an in-situ crystallization catalyst.

[0048] The directing agent described in the present invention is not particularly limited, and a common directing agent can be used. For example, the molar ratio of the directing agent is (14-16) SiO2: (0.7-1.3) Al2O3: (14-16) Na2O: (300-330) H2O, and its preparation method refers to the method described in CN1081425A.

[0049] In the present invention, the spray microspheres are subjected to calcination, and the calcination process conditions are well known to those skilled in the art, for example, calcination at 600-1000°C for 1-3 hours, which is not particularly limited in the present invention. The spray microspheres can be calcined at 920-1000°C for 1-3 hours to obtain high-earth microspheres; or calcined at 600-900°C for 1-3 hours to obtain partial-earth microspheres. The preparation method disclosed in the present invention can prepare the spray microspheres of the in-situ crystallization product, which can be high-earth microspheres, partial-earth microspheres, or a mixture of high-earth microspheres and partial-earth microspheres.

[0050] The preparation method of the heavy oil type in-situ crystallization catalyst described in the present invention is preferably that, based on the catalyst weight as 100%, the sodium oxide content is ≤1%, based on RE2O3, the rare earth content is 1-15%, more preferably 2-12%, and based on P2O5, the phosphorus content is 0-5%, more preferably 0.1-3%.

[0051] The preparation method of the heavy oil type in-situ crystallization catalyst described in the present invention, wherein preferably, the kaolin is selected from at least one of hard kaolin, soft kaolin and coal ash, and further preferably, the particle size of the kaolin is 2.5-3.5 μm, the crystalline kaolin content is higher than 80wt%, the iron oxide is lower than 1.7wt%, and the sum of sodium oxide and potassium oxide is lower than 0.5wt%.

[0052] In the preparation method of the heavy oil type in-situ crystallization catalyst of the present invention, preferably, a binder is added when preparing the mixed slurry in step (1), and more preferably, the binder is selected from one or more of sodium silicate, silica sol, aluminum sol, and pseudo-boehmite, and the amount added is 2% to 10% of the mass of kaolin. The main function of the binder is to act as a dispersant or to improve the wear resistance of the catalyst.

[0053] The method for preparing a heavy oil-based in-situ crystallization catalyst of the present invention is preferably such that, in step (1), the solid content of the mixed slurry is 30-50wt%, the particle size of the kaolin spray microspheres is 20-110μm, the calcination conditions are: 600-1000°C for 1-3 hours, and the crystallization conditions are: 90-110°C for 18-36 hours.

[0054] The preparation method of the heavy oil type in-situ crystallization catalyst of the present invention is preferably that in step (2), the conditions of the exchange and calcination are: the exchange is carried out at pH 3-6 and temperature 60-100°C; the calcination temperature is 500-800°C, the time is 0.5-2 hours, and the water vapor amount is 0-100%.

[0055] The method for preparing a heavy oil-based in-situ crystallization catalyst of the present invention is preferably such that in step (2), the ammonium salt is selected from one or more of ammonium sulfate, ammonium chloride, ammonium nitrate, and ammonium phosphate, and ammonium chloride and / or ammonium nitrate are further preferred; the rare earth is selected from one or more of rare earth chloride and rare earth nitrate; the phosphorus is selected from one or more of diammonium hydrogen phosphate, diammonium dihydrogen phosphate, ammonium phosphate, and ammonium hydrogen phosphate, and diammonium hydrogen phosphate and / or ammonium phosphate are further preferred.

[0056] The present invention discloses a more specific technical solution for preparing in-situ crystallized products of kaolin microspheres containing silicon-aluminum materials: a mixed slurry is prepared from silicon-aluminum materials and kaolin as raw materials, and its solid content is 30-50%. Microspheres with a particle size of 20-110 μm are obtained by spray drying. The microspheres are calcined at 600-1000° C. for 1-3 hours, mixed with water glass, alkaline solution and directing agent, crystallized at 90-110° C. for 18-36 hours, filtered, washed and dried.

[0057] The preparation method of the catalyst disclosed in the present invention, the exchange and roasting of the crystallized product are general technologies for the preparation of in-situ crystallized catalysts, and the present invention has no special limitations. In the exchange process of the crystallized product, the exchange material can be introduced simultaneously or separately, and the exchange material is one or more of ammonium salts, rare earths and phosphorus; the number of exchanges is not limited, and a single or multiple exchanges can be performed. When multiple exchanges are performed, the exchange materials for each exchange can be the same or different; roasting can be performed under 0-100% water vapor conditions, and the roasting process can be a single roasting or multiple roastings; the exchange and roasting processes can be performed as long as they can meet the requirements of the final catalyst.

[0058] The beneficial effects of the present invention are as follows:

[0059] The catalyst provided by the present invention contains a silicon-aluminum material, which has a high pore volume, a large specific surface area, a double pore distribution, a high thermal stability, a high acid content, and contains a B acid center. The introduction of the silicon-aluminum material improves the pore structure and acid distribution of the in-situ crystallization catalyst carrier, and the prepared in-situ crystallization catalytic cracking catalyst has the characteristics of high pore volume, strong heavy oil conversion ability, and high gasoline yield.

[0060] The catalyst preparation method provided by the present invention adopts the silicon-aluminum material to prepare kaolin spray microspheres, and then obtains a heavy oil type in-situ crystallization catalyst through in-situ crystallization, exchange and calcination steps, which has a higher pore volume, stronger heavy oil conversion performance and higher gasoline yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 This is the XRD spectrum of the silicon-alumina and industrial pseudo-boehmite materials prepared in Example 3. Figure 1It shows that the prepared silicon-alumina material has a pseudo-boehmite crystal phase structure, but its crystallinity is lower than that of industrial pseudo-boehmite.

[0062] Figure 2 This is a SEM picture of the silicon-aluminum material prepared in Example 3. The silicon-aluminum material is formed by stacking short nanorods, and two types of pore distributions, mesopores and macropores, can be clearly observed.

[0063] Figure 3 This is the BJH pore distribution curve of the silicon-aluminum material AS-3 prepared in Example 3. Figure 3 It shows that the silicon-aluminum material has a dual pore distribution of 2-40nm and 70-300nm, respectively, while the comparative industrial pseudo-boehmite material has only a single pore distribution between 2-4nm, and the pore diameter is 3.4nm; AS-7 and AS-8 are the BJH pore distribution curves of the materials prepared in Comparative Example 1 and Comparative Example 2, respectively. DETAILED DESCRIPTION

[0064] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions, and the unspecified % is weight %.

[0065] Analytical methods

[0066] In each embodiment, the content of Na2O, A12O3 and SiO2 in the product was determined by X-ray fluorescence method (see "Analysis Methods in Petrochemical Industry (RIPP Experimental Methods)", edited by Yang Cuiding et al., Science Press, published in 1990). The specific surface area and pore structure were measured by low-temperature nitrogen adsorption-desorption method, and the pore distribution curve was calculated by BJH method. Scanning electron microscopy (SEM) was characterized by ULTRA-Plus field emission scanning electron microscope of Zeiss, Germany.

[0067] Pyridine adsorption infrared spectroscopy (Py-FTIR) was used to characterize the acid type of the sample using a TENSOR-27 Fourier transform infrared spectrometer produced by Bruker Corporation of the United States. 10 mg of the sample was pressed into a tablet and placed in an in-situ detection cell. The surface was cleaned in a vacuum environment at 350°C for two hours, and then infrared analysis was performed.

[0068] Pore ​​volume determination by water drop method: Take about 80g of catalyst sample and place it in an evaporating dish, burn it at 480℃ for 1 hour, take it out and cool it in a desiccator, take 20g of sample and add it to a conical flask, accurate to 0.1g. Add distilled water to the conical flask through a burette. With the addition of water, the fluidity of the catalyst deteriorates. Use a glass rod to stir and shake it continuously until the sample loses fluidity and all aggregates together. Record the water consumption and use Vp=V / m to calculate the sample pore volume. Vp-sample pore volume, ml / g; V-consumed titration water volume, ml; m-sample mass, g.

[0069] Source of raw materials

[0070] Aluminum chloride, sodium aluminate, aluminum sulfate, aluminum nitrate, propanol, ethanol, ethylene glycol, butanol, butanediol, ammonium nitrate, ammonium sulfate, ammonium chloride, methyl orthosilicate, ethyl orthosilicate, and sodium silicate are analytical reagents and are produced by Sinopharm Chemical Reagent Co., Ltd.

[0071] Sodium silicate, hydrochloric acid, ammonia water, and industrial pseudo-boehmite were provided by PetroChina Lanzhou Petrochemical Catalyst Plant.

[0072] NaY zeolite directing agent, produced by the catalyst plant of Lanzhou Petrochemical Company;

[0073] Kaolin, an industrial product of China Kaolin Corporation, will be reduced by 16.57%;

[0074] Pseudo-boehmite, produced by Shanxi Aluminum Plant, is reduced by 37.69%.

[0075] Example 1

[0076] Silicon aluminum material preparation

[0077] Prepare 59g / L aluminum sulfate solution (alumina, the same below) and 44g / L sodium aluminate solution, and heat them to 57°C and 62°C respectively. Then, add the aluminum sulfate and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 59°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value = 6.4. Continue stirring for 30 minutes after the feeding is completed. Then, add water glass according to SiO2:Al2O3=0.39:1. After the water glass is added, add propanol at 6.2 times the weight of alumina. Then, continue stirring and aging at 59°C for 1.4 hours, then raise the temperature to 98°C, add low alumina to adjust the pH value to 8.1, and stir and age at 98°C for 1.3 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium sulfate: solid precipitate (dry basis): water = 0.3:1:7, and ion exchange is performed at 93°C to remove sodium ions. The exchange is repeated twice, each time for 0.8h. After each exchange, it is washed and filtered, and then dried at 120°C for 18h to obtain the silicon-aluminum material AS-1 provided by the present invention, and the elemental analysis chemical composition is 0.17Na2O:71.7Al2O3:28.2SiO2.

[0078] Catalyst preparation

[0079] 3000g kaolin (dry basis), based on the mass of kaolin, was added with 2% water glass, 6% silica sol, 2% AS-1, and deionized water to prepare a mixed slurry with a solid content of 38%, and 3267g of kaolin spray microspheres with a particle size of 20 to 110μm were obtained. A portion of the microspheres was calcined at 960℃ for 2.5 hours to obtain kaolin microspheres GT-1, and another portion was calcined at 830℃ for 1.5 hours to obtain partial soil microspheres PT-1.

[0080] Take 800g of GT-1 high soil microspheres, 200g of partial soil microspheres PT-1, 6470ml of water glass, 2450ml of 14wt% sodium hydroxide solution, and 870ml of directing agent, stir for 30 minutes, and then put the mixed solution into a stainless steel reactor, heat it to 94℃ and keep it at a constant temperature for 32h. After the crystallization is completed, remove the white powder in the solution by sedimentation washing, and then filter, wash and dry the filter cake to obtain the in-situ crystallization product. X-ray diffraction determination shows that it contains 35% NaY zeolite.

[0081] 400 g of crystallized product, ammonium sulfate and deionized water were added into a stainless steel kettle under stirring, with ammonium sulfate / crystallized product=0.40, and exchanged at pH=3.0-3.5 and 90°C for 2.0 hours. The filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain a cross-linked material; the cross-linked material was roasted at 570°C and a water vapor introduction rate of 38% for 1.8 hours to obtain a roasted material; the roasted material was exchanged once with rare earth chloride, and the exchange conditions were: rare earth / a roasted material=0.08, pH=3.0-3.5, and a reaction mixture was added under the conditions of 1.5% sodium hydroxide solution and 2.0% sodium hydroxide solution. 3.5, the temperature is 90°C, the time is 1.5 hours, the exchanged material is filtered, washed and dried to obtain the second cross material; the second cross material is roasted at 610°C and the water vapor introduction amount is 80% for 2 hours to obtain the second roasted material; the second roasted material is first exchanged with ammonium nitrate, ammonium nitrate / second roasted material=0.50, pH=3.3-4.8, after 1.2 hours of exchange at 87°C, the product is filtered, washed with water and dried to obtain the catalyst CAT-1 with a Na2O content of 0.48% and a rare earth content of 6.52%.

[0082] Example 2

[0083] Silicon aluminum material preparation

[0084] Prepare 73g / L aluminum nitrate solution and 58g / L sodium aluminate solution, and heat them to 52°C and 59°C respectively. Then, add the aluminum nitrate and sodium aluminate solutions into the reactor in parallel with stirring. Keep the gelling temperature at 55°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value is 6.6. Continue stirring for 25 minutes after the feeding is completed. Then, add sodium silicate solution according to SiO2:Al2O3=0.26:1. After the sodium silicate is added, add ethanol at 7.7 times the weight of alumina. Then, continue stirring and aging at 55°C for 2.1 hours, then raise the temperature to 91°C, add ammonia solution to adjust the pH value to 8.9, and stir and age at 91°C for 1.1 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to the ratio of ammonium chloride: solid precipitate (dry basis): water = 0.6:1:9, hydrochloric acid is added to adjust the pH to 2.5, and ion exchange is performed at 75°C to remove sodium ions, and the exchange is repeated once, each time for 0.9h. After the exchange, it is washed and filtered, and then dried at 100°C for 30h to obtain the silicon-aluminum material AS-2 provided by the present invention, and the elemental analysis chemical composition is 0.03Na2O:79.4Al2O3:20.6SiO2.

[0085] Catalyst preparation

[0086] 3000g kaolin (dry basis), based on the mass of kaolin, 4% water glass, 6% AS-2, and deionized water were added to prepare a mixed slurry with a solid content of 35%, and 3231g of kaolin spray microspheres with a particle size of 20-110μm were obtained. A portion of the microspheres was calcined at 940℃ for 2.0 hours to obtain GT-2 kaolin microspheres, and another portion was calcined at 790℃ for 2.6 hours to obtain PT-2 kaolin microspheres.

[0087] 1000g of GT-2 high soil microspheres were mixed with 7100ml of water glass, 3410ml of 14 wt% sodium hydroxide solution, and 117ml of directing agent. After stirring for 30 minutes, the mixture was put into a stainless steel reactor and heated to 98°C for 28h of constant temperature crystallization. After the crystallization was completed, the white powder in the solution was removed by sedimentation washing, and then the filter cake was filtered, washed, and dried to obtain an in-situ crystallization product. X-ray diffraction determined that it contained 30% NaY zeolite.

[0088] 800g of crystallized product, ammonium chloride, ammonium sulfate and deionized water were added into a stainless steel kettle under stirring, with ammonium chloride / crystallized product = 0.35, ammonium nitrate / crystallized product = 0.25, and exchanged at pH = 3.0-3.5, 90°C for 1.1 hours, and the filtrate was filtered out. The filter cake was washed with deionized water and dried to obtain a cross-linked material; the cross-linked material was roasted at 630°C and a water vapor introduction rate of 70% for 2 hours to obtain a roasted material; the roasted material was exchanged once with rare earth nitrate, and the exchange conditions were: rare earth / a roasted material = 0.06, pH = 3.4-3.9, temperature 92°C, time 1.3 hours, and the exchanged material was The method comprises the following steps: filtering, washing and drying to obtain a second cross-linked material; calcining the second cross-linked material at 650° C. and 85% water vapor introduction for 1.6 hours to obtain a second roasted material; exchanging the second roasted material with ammonium sulfate, ammonium sulfate / second roasted material=0.42, pH=3.5-4.0, exchanging at 88° C. for 1.5 hours, introducing diammonium hydrogen phosphate into the exchange solution, adding phosphorus / second roasted material=0.03, pH=4.0-4.5, and continuing to exchange at 96° C. for 1.4 hours. The exchange product is filtered, washed with water and dried to obtain a catalyst CAT-2 having a Na2O content of 0.38%, a rare earth content of 4.23% and a phosphorus content of 2.49%.

[0089] Example 3

[0090] Silicon aluminum material preparation

[0091] Prepare 120g / L aluminum sulfate solution and 50g / L sodium aluminate solution, and heat them to 60°C and 65°C respectively. Then, add the aluminum sulfate and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 63°C during the feeding process. Control the feeding speed of the two solutions so that the gelling pH value is 7.5. Continue stirring for 15 minutes after the feeding is completed. Then, add methyl orthosilicate solution according to SiO2:Al2O3=0.15:1. After the addition of methyl orthosilicate is completed, add propanol at 3 times the weight of alumina. Then, continue stirring and aging at 63°C for 1.0 hour, then raise the temperature to 95°C, add sodium aluminate solution to adjust the pH value to 8.5, and stir and age at 95°C for 2.0 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium chloride: solid precipitate (dry basis): water = 1:0.4:7, and ion exchange is performed at 90°C to remove sodium ions therein. The exchange is repeated twice, each time for 1.0h. After each exchange, the product is washed and filtered, and then dried at 120°C for 15h to obtain the silicon-aluminum material AS-3 provided by the present invention, and the elemental analysis chemical composition is 0.03Na2O:86.6Al2O3:13.4SiO2.

[0092] Catalyst preparation

[0093] 3000g of kaolin (dry basis), based on the mass of kaolin, 2% water glass, 5% AS-3, and deionized water were added to prepare a mixed slurry with a solid content of 40%, and 3109g of kaolin spray microspheres with a particle size of 20-110μm were obtained. A portion of the microspheres was calcined at 970℃ for 1.5 hours to obtain GT-3 kaolin microspheres, and another portion was calcined at 810℃ for 2.2 hours to obtain PT-3 kaolin microspheres.

[0094] Take 400g of high-earth microspheres GT-3 and 600g of partial-earth microspheres PT-3, mix them with 3245ml of water glass, 746ml of 14wt% sodium hydroxide solution, and 450ml of directing agent, stir for 30 minutes, put the mixed solution into a stainless steel reactor, heat it to 100℃ and keep it at a constant temperature for 22h. After the crystallization is completed, remove the white powder in the solution by sedimentation washing, and then filter, wash and dry the filter cake to obtain the in-situ crystallization product. X-ray diffraction determination shows that it contains 51% NaY zeolite.

[0095] 500 g of the crystallized product prepared in Example 3, ammonium chloride, ammonium sulfate and deionized water were added to a stainless steel kettle under stirring, with ammonium chloride / crystallized product = 0.20, ammonium sulfate / crystallized product = 0.50, and exchanged at pH = 4.0-4.5 and 83° C. for 0.9 hour. The filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain a cross-linked material; the cross-linked material was roasted at 660° C. and a water vapor introduction rate of 90% for 1.9 hours to obtain a roasted material; the roasted material was exchanged once with rare earth nitrate, and the exchange conditions were: rare earth nitrate / a roasted material = 0.06, pH=3.3-3.8, temperature is 91°C, time is 1.2 hours, the exchanged material is filtered, washed and dried to obtain a second cross material; the second cross material is roasted at 560°C and a water vapor introduction amount of 75% for 1.8 hours to obtain a second roasted material; the second roasted material is exchanged with rare earth nitrate, rare earth / second roasted material=0.05, pH=3.5-4.0, exchanged at 91°C for 1.3 hours, the exchanged product is filtered, washed with water and dried to obtain a catalyst CAT-3 with a Na2O content of 0.41% and a rare earth content of 8.33%.

[0096] Example 4

[0097] Silicon aluminum material preparation

[0098] Prepare 82g / L aluminum chloride solution and 107g / L sodium aluminate solution, and heat them to 48°C and 54°C respectively. Then, add the aluminum chloride and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 51°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value = 6.0. Continue stirring for 40 minutes after the feeding is completed. Then, add water glass according to SiO2:Al2O3=0.11:1. After the water glass is added, add propylene glycol at 4.7 times the weight of alumina. Then, continue stirring and aging at 51°C for 0.7 hour, then raise the temperature to 86°C, add ammonia solution to adjust the pH value to 9.2, and stir and age at 86°C for 1.5 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium nitrate: solid precipitate (dry basis): water = 0.5:1:10, and ion exchange is carried out at 85°C to remove sodium ions therein, and the exchange is carried out for 1.0h. After each exchange, it is washed and filtered, and then dried at 145°C for 12h to obtain the silicon-aluminum material AS-4 provided by the present invention, and the elemental analysis chemical composition is 0.08Na2O:90.0Al2O3:9.9SiO2.

[0099] Catalyst preparation

[0100] 3000g kaolin (dry basis), based on the mass of kaolin, was added with 4% water glass, 4% aluminum sol, and 4% AS-4, and deionized water to prepare a mixed slurry with a solid content of 38%, and 3069g of kaolin spray microspheres with a particle size of 20 to 110μm were obtained. A portion of the microspheres was calcined at 930℃ for 2.4 hours to obtain kaolin microspheres GT-4, and another portion was calcined at 750℃ for 2.3 hours to obtain partial soil microspheres PT-4.

[0101] Take 900g of high-earth microspheres GT-3, 100g of partial-earth microspheres PT-3, 2867ml of water glass, 487ml of 14 wt% sodium hydroxide solution, and 415ml of directing agent, mix them, stir for 30 minutes, put the mixed solution into a stainless steel reactor, heat it to 95℃ and keep it at a constant temperature for 25h. After the crystallization is completed, remove the white powder in the solution by sedimentation washing, and then filter, wash and dry the filter cake to obtain the in-situ crystallization product. X-ray diffraction determination shows that it contains 38% NaY zeolite.

[0102] 500g of crystallized product, ammonium nitrate and deionized water were added into a reaction kettle under stirring, ammonium nitrate / crystallized product=0.50, exchanged at pH=3.0-3.5, 97°C for 0.7 hour, filtered to remove the filtrate, washed the filter cake with deionized water and dried to obtain a first cross-linked material; the first cross-linked material was exchanged with rare earth chloride, the addition ratio was rare earth / first cross-linked material=0.06, pH=3.5-4.0, exchanged at 92°C for 1.3 hours, the exchanged product was filtered, washed with water and dried to obtain a second cross-linked material; the second cross-linked material was roasted at 620°C without water vapor for 1.7 hours to obtain a first roasted material; the first roasted material was exchanged with ammonium nitrate once again, and the exchange conditions were: ammonium nitrate / first roasted material=0.45, pH=4.0 ~4.5, the temperature is 88℃, the time is 1.8 hours, the exchanged material is filtered, washed and dried to obtain the third cross material; the third cross material is roasted at 720℃, the water vapor introduction amount is 90% for 1.6 hours to obtain the second roasted material; the second roasted material is first exchanged with ammonium chloride, ammonium chloride / second roasted material=0.3, pH=3.8~4.3, after exchanging at 97℃ for 0.7 hour, rare earth nitrate is added to the exchange solution, the addition ratio is rare earth / second roasted material=0.06, pH=3.3~3.8, and the exchange is continued at 90℃ for 1.1 hours, the exchange product is filtered, washed with water and dried to obtain the catalyst CAT-4 with a Na2O content of 0.37% and a rare earth content of 9.84%.

[0103] Example 5

[0104] Silicon aluminum material preparation

[0105] Prepare 146g / L aluminum nitrate solution and 26g / L sodium aluminate solution, and heat them to 45°C. Then, add the aluminum nitrate and sodium aluminate solutions into the reactor in parallel with stirring. Keep the gelling temperature at 45°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value is 7.8. Continue stirring for 45 minutes after the feeding is completed. Then, add tetraethyl orthosilicate solution according to SiO2:Al2O3=0.34:1. After the addition of tetraethyl orthosilicate is completed, add butanol at 1.7 times the weight of alumina. Then, continue stirring and aging at 45°C for 2.4 hours, then raise the temperature to 81°C, add sodium hydroxide solution to adjust the pH value to 10.0, and stir and age at 81°C for 2.3 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed at a ratio of solid precipitate (dry basis): water = 1:5, and ion exchange is performed at 80°C to remove sodium ions therein. The exchange is repeated once, each time for 0.6h. After each exchange, the product is washed and filtered, and then dried at 160°C for 11h to obtain the silicon-aluminum material AS-5 provided by the present invention, and the elemental analysis chemical composition is 0.03Na2O:74.3Al2O3:25.4SiO2.

[0106] Catalyst preparation

[0107] 3000g kaolin (dry basis), based on the mass of kaolin, added 1% water glass, 6% aluminum sol, 10% AS-5, and added deionized water to prepare a mixed slurry with a solid content of 33%, and 3117g of kaolin spray microspheres with a particle size of 20-110μm were obtained. A portion of the microspheres was calcined at 950℃ for 2.2 hours to obtain GT-5 kaolin microspheres, and another portion was calcined at 730℃ for 1.8 hours to obtain PT-5 kaolin microspheres.

[0108] Take 700g of high-earth microspheres GT-5 and 300g of partial-earth microspheres PT-5, mix them with 4125ml of water glass, 1347ml of 14wt% sodium hydroxide solution, and 412ml of directing agent, stir for 30 minutes, put the mixed solution into a stainless steel reactor, heat it to 99℃ and keep it at a constant temperature for 30h. After the crystallization is completed, remove the white powder in the solution by sedimentation washing, and then filter, wash and dry the filter cake to obtain the in-situ crystallization product. X-ray diffraction determination shows that it contains 46% NaY zeolite.

[0109] 600 g of crystallized product, ammonium sulfate, rare earth chloride and deionized water were added into a stainless steel kettle under stirring, with ammonium sulfate / crystallized product = 0.35, rare earth / crystallized product = 0.04, and exchanged for 1.2 hours at pH = 4.5-5.0 and 91° C., the filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain a cross-linked material; the cross-linked material was roasted at 580° C. and a water vapor introduction rate of 80% for 1.8 hours to obtain a roasted material; the roasted material was exchanged once with rare earth nitrate, and the exchange conditions were: rare earth / a roasted material = 0.03, pH=3.0~3.3, temperature is 96℃, time is 1.3 hours, the exchanged material is filtered, washed and dried to obtain the second cross material; the second cross material is roasted at 670℃ and 100% water vapor introduction for 1.9 hours to obtain the second roasted material; the second roasted material is first exchanged with ammonium nitrate, ammonium nitrate / second roasted material=0.40, pH=3.5~4.0, after exchanging at 83℃ for 1.7 hours, the exchange product is filtered, washed with water and dried to obtain the catalyst CAT-5 with a Na2O content of 0.51% and a rare earth content of 4.98%.

[0110] Example 6

[0111] Silicon aluminum material preparation

[0112] Prepare 101g / L aluminum sulfate solution and 73g / L sodium aluminate solution, and heat them to 46°C and 52°C respectively. Then, add the aluminum sulfate and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 48°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value = 7.3. Continue stirring for 20 minutes after the feeding is completed. Then, add water glass according to SiO2:Al2O3=0.06:1. After the water glass is added, add butanediol at 3.2 times the weight of alumina. Then, continue stirring and aging at 48°C for 1.7 hours, then raise the temperature to 94°C, add water glass solution to adjust the pH value to 9.6, and stir and age at 94°C for 0.6 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium nitrate: solid precipitate (dry basis): water = 0.25:1:6, and ion exchange is performed at 87°C to remove sodium ions therein. The exchange is repeated once, each time for 0.9 h. After each exchange, the product is washed and filtered, and then dried at 140°C for 14 h to obtain the silicon-aluminum material AS-6 provided by the present invention, and the elemental analysis chemical composition is 0.11Na2O:94.2Al2O3:5.7SiO2.

[0113] 3000g kaolin (dry basis), based on the mass of kaolin, was added with 2% water glass, 3% silica sol, 8% AS-6, and deionized water to prepare a mixed slurry with a solid content of 42%, and 3073g of kaolin spray microspheres with a particle size of 20 to 110μm were obtained. A portion of the microspheres was calcined at 920℃ for 3.0 hours to obtain GT-6 kaolin microspheres, and another portion was calcined at 650℃ for 2.8 hours to obtain PT-6 kaolin microspheres.

[0114] Take 200g of high-earth microspheres GT-6 and 800g of partial-earth microspheres PT-6, mix them with 3709ml of water glass, 1721ml of 14 wt% sodium hydroxide solution, and 857ml of directing agent, stir for 30 minutes, and then put the mixed solution into a stainless steel reactor, heat it to 105℃ and keep it at constant temperature for 20h for crystallization. After the crystallization is completed, remove the white powder in the solution by sedimentation washing, and then filter, wash and dry the filter cake to obtain the in-situ crystallization product. X-ray diffraction determination shows that it contains 56% NaY zeolite.

[0115] 600g of crystallized product, ammonium sulfate, ammonium chloride, ammonium nitrate and deionized water were added into a stainless steel kettle under stirring, with ammonium sulfate / crystallized product=0.30, ammonium chloride / crystallized product=0.30, ammonium nitrate / crystallized product=0.15, and exchanged at pH=4.0-4.5, 97°C for 1.5 hours, and the filtrate was filtered to remove the filtrate, and the filter cake was washed with deionized water and dried to obtain a cross-material; the cross-material was then exchanged with ammonium nitrate and rare earth nitrate, and the exchange conditions were: ammonium nitrate / cross-material=0.25, rare earth nitrate / cross-material=0.06, pH=3.5-4.0, temperature of 92°C, and time of 1.6 hours. The exchanged materials were filtered, washed and dried to obtain a second cross-material; the second cross-material was roasted at 540°C and a steam introduction amount of 95% for 1.9 hours to obtain a roasted material; The roasted material is exchanged with rare earth chloride once again, and the exchange conditions are: rare earth chloride / first roasted material=0.04, pH=3.3-3.8, temperature is 86°C, and time is 1.2 hours. The exchanged material is filtered, washed, and dried to obtain a third roasted material; the third roasted material is roasted at 630°C without water vapor for 2 hours to obtain a second roasted material; the second roasted material is first exchanged with ammonium sulfate, ammonium sulfate / second roasted material=0.30, pH=4.3-4.8, and after exchanging at 94°C for 1.2 hours, ammonium hydrogen phosphate is added to the exchange solution, and the addition ratio is phosphorus / second roasted material=0.03, pH=3.0-3.5, and the exchange is continued at 94°C for 0.8 hours. The exchange product is filtered, washed with water, and dried to obtain a catalyst CAT-6 with a Na2O content of 0.39%, a rare earth content of 7.52%, and a phosphorus content of 2.65%.

[0116] Comparative Example 1

[0117] Pseudo-boehmite was used to replace AS-3, and kaolin spray microspheres were prepared according to the catalyst preparation method in Example 3. The comparative catalyst CAT-7 was also prepared according to the catalyst preparation method in Example 3.

[0118] Comparative Example 2

[0119] Comparative Example 2 was prepared according to the preparation process of CN201510864343.7.

[0120] Aluminum sulfate and sodium aluminate are used as raw materials, and the gel is formed at 63°C in parallel, and the pH value of the gel is controlled to be 7.5. At the same time, methyl silicate solution is added online according to SiO2:Al2O3=0.15:1, and mixed with the gel slurry in parallel. After the raw materials are added, the slurry is heated to 90°C and aged for 2.0 hours. After filtering and washing, the obtained product is mixed with ammonium chloride: solid precipitate (dry basis): water=1:0.4:10, and ion exchange is carried out at 90°C to remove sodium ions. The exchange is repeated twice, each time for 1.0h, and after each exchange, it is washed and filtered, and then dried at 120°C for 15h, and the comparative silicon aluminum material AS-7 is obtained, and the elemental analysis chemical composition is 0.04Na2O:86.8Al2O3:13.2SiO2.

[0121] AS-7 was used instead of AS-3, and kaolin spray microspheres were prepared according to the catalyst preparation method in Example 3. The comparative catalyst CAT-8 was also prepared according to the catalyst preparation method in Example 3.

[0122] Comparative Example 3

[0123] Silicon aluminum material was prepared according to the preparation process of CN201710382520.7.

[0124] A small amount of deionized water was added to the beaker, and then water glass (250 g / L, silicon oxide) and sodium aluminate solution (107 g / L, aluminum oxide) were added in parallel at 51°C by strong stirring, and the flow rate was controlled so that the water glass and sodium aluminate were added at the same time, and the pH value was 13.0; then 82 g / l of aluminum chloride solution was added, and the end point pH value of the slurry system was controlled to be 9.2, and then the product was treated at a constant temperature for 1.5 hours at 86°C. After filtering and washing, the obtained solid precipitate was mixed according to ammonium nitrate: solid precipitate (dry basis): water = 0.5:1:10, and ion exchange was performed at 85°C to remove sodium ions therein, and the exchange was performed for 1.0h. After each exchange, it was washed and filtered, and then dried at 145°C for 12h, and the comparative silicon aluminum material AS-8 was obtained, and the elemental analysis chemical composition was 0.10Na2O:90.2Al2O3:9.7SiO2.

[0125] AS-8 was used instead of AS-4, and kaolin spray microspheres were prepared according to the catalyst preparation method in Example 4. Comparative catalyst CAT-9 was also prepared according to the catalyst preparation method in Example 4.

[0126] Table 1 provides the pore structure data and pyridine infrared acidity data of samples AS-1 to AS-6 prepared in Examples 1-6, as well as the comparative materials industrial pseudo-boehmite and AS-7 and AS-8.

[0127] Table 1 Physicochemical properties of different samples

[0128]

[0129]

[0130] Table 2 shows the changes in the micro-reactivity of catalysts CAT-1 to CAT-6 prepared from the in-situ crystallization products of Examples 1 to 6 and catalysts CAT-7 to CAT-9 prepared from the in-situ crystallization products of Comparative Examples 1 to 3.

[0131] Table 2 Comparative data of CAT-1~CAT-6 and CAT-7~CAT-8

[0132]

[0133] In Table 2, the test conditions of the micro-reaction activity* are: 800°C, 17 hours, and 100% water vapor aging.

[0134] From the data comparison in Table 2, it can be seen that the pore volume and 17-hour micro-reaction activity of the in-situ crystallization catalyst prepared by the preparation method of the present invention are higher than those of the catalyst prepared by the comparative example.

[0135] Test Example 1

[0136] Catalyst Evaluation:

[0137] Catalyst CAT-3 prepared in Example 3 and catalysts CAT-7 and CAT-8 prepared in Comparative Examples 1 and 2 were evaluated for catalyst performance using a fixed fluidized bed apparatus, and the raw material used was the raw material of the 3 million tons / year heavy oil catalytic cracking unit of Lanzhou Petrochemical, and the properties of the raw material are shown in Table 3. Before the catalyst evaluation, it was aged at 800°C and 100% steam for 10 hours; and the catalytic cracking reaction conditions were: reaction temperature 500°C, catalyst-oil mass ratio 6.0, i.e., the conditions of "reaction performance **" in Table 4. The evaluation results are listed in Table 4.

[0138] Table 3 Properties of feedstock oil used for catalyst selectivity evaluation

[0139]

[0140] Table 4 Reaction performance evaluation of different catalysts

[0141]

[0142]

[0143] The data in Table 4 show that, compared with the existing catalysts, the catalyst provided by the present invention has higher activity, lower heavy oil yield, higher gasoline yield and total liquid yield. Compared with the comparative catalysts CAT-7 and CAT-8, the catalyst prepared in Example 3 has a heavy oil reduction of 1.66 and 0.97 percentage points, a gasoline yield increase of 1.86 and 1.17 percentage points, and a total liquid yield increase of 2.20 and 1.37 percentage points, respectively. For the catalytic cracking unit, the total liquid yield only increases by 0.5 percentage points, which can bring huge economic benefits to the oil refining enterprise.

[0144] Test Example 2

[0145] The same evaluation conditions and raw materials as those in Experimental Example 1 were used to evaluate the catalyst performance of CAT-4 prepared in Example 4 and CAT-9 prepared in Comparative Example 3 in the riser, and the results are listed in Table 5. The catalyst was aged at 800°C and 100% steam for 10 hours before evaluation; and the catalytic cracking reaction conditions were: reaction temperature 500°C, catalyst-oil mass ratio 6.0, i.e., the conditions of "Reaction Performance*" in Table 5.

[0146] Table 5 Reaction performance evaluation of different catalysts

[0147]

[0148] The data in Table 5 show that, under the same preparation process, the catalyst provided by the present invention has higher activity, stronger heavy oil conversion ability and higher gasoline yield compared with the same amount of functional components added. Compared with the comparative catalyst CAT-9, the heavy oil content of CAT-4 decreased by 0.75 percentage points and the total liquid yield increased by 0.84 percentage points.

[0149] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the protection scope of the present invention.

Claims

1. A heavy oil type in-situ crystallization catalyst, characterized in that: The raw material of kaolin microspheres for preparing the catalyst contains a silicon-aluminum material, which has a pseudo-boehmite structure, and its anhydrous chemical expression is (0-0.2)Na2O: (4-30)SiO2: (70-96)Al2O3, which has a double pore distribution of 2-40 nm and 70-300 nm, and a specific surface area of ​​more than 500 m 2 / g, and not more than 650 m 2 / g, the pore volume is 2.1-2.8 ml / g, and the ratio of pyridine infrared B acid content to L acid content measured at 200°C is 0.14-0.

38.

2. The heavy oil type in-situ crystallization catalyst according to claim 1, characterized in that: The amount of silicon-aluminum material added to the kaolin microsphere raw material is 1-10% of the mass of kaolin.

3. The heavy oil type in-situ crystallization catalyst according to claim 2, characterized in that: The amount of silicon-aluminum material added to the raw material of kaolin microspheres is 2-8% of the mass of kaolin.

4. The heavy oil type in-situ crystallization catalyst according to claim 1, characterized in that: The silicon-aluminum material is prepared by the following steps: (1) Preheat the acidic aluminum source and sodium aluminate solution to 45-70°C respectively, add them into the reactor in parallel, maintain the temperature at 45-70°C, stir and react, and the pH value of the reaction is 6-8; (2) Add silicon source at a weight ratio of SiO2: Al2O3 = 0.05-0.43:1, and add alcohol solvent and stir evenly for primary aging, maintaining the primary aging temperature at 45-70°C and the primary aging pH value at 6-8; (3) Raising the temperature to 80-100°C, adding an alkaline solution to adjust the pH value to 8.5-10.0, and performing secondary aging under stirring to obtain a solid precipitate; (4) Filter, wash, exchange and dry the obtained solid precipitate.

5. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The acidic aluminum source is one or more of aluminum nitrate, aluminum sulfate and aluminum chloride.

6. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The concentration of the acidic aluminum source is 50-150 g / L in terms of aluminum oxide, and the concentration of the sodium metaaluminate solution is 20-130 g / L in terms of aluminum oxide.

7. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The silicon source is selected from one or more of sodium silicate and silicate compounds.

8. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The silicon source is selected from water glass.

9. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: In step (2), the silicon source and the alcohol solvent are added simultaneously, or the silicon source is added first and then the alcohol solvent.

10. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The acidic aluminum source is based on the weight of aluminum oxide, and the added amount of the alcohol solvent is 1-10 times that of the acidic aluminum source.

11. The heavy oil type in-situ crystallization catalyst according to claim 10, characterized in that: The acidic aluminum source is based on the weight of aluminum oxide, and the added amount of the alcohol solvent is 2-5 times that of the acidic aluminum source.

12. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The alcohol solvent is a compound in which hydrogen atoms in saturated aliphatic hydrocarbons and / or alicyclic hydrocarbons are replaced by hydroxyl groups.

13. The heavy oil type in-situ crystallization catalyst according to claim 12, characterized in that: The alcohol solvent is a C1-C8 monohydric alcohol, dihydric alcohol or trihydric alcohol.

14. The heavy oil type in-situ crystallization catalyst according to claim 12, characterized in that: The alcohol solvent is a C2-C4 alcohol.

15. The heavy oil type in-situ crystallization catalyst according to claim 12, characterized in that: The alcohol solvent is selected from one or more of ethanol, ethylene glycol, propanol, glycerol, butanol and butanediol.

16. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The time of the first aging is 0.5-3 h, and the time of the second aging is 0.5-3 h.

17. The heavy oil type in-situ crystallization catalyst according to claim 4, characterized in that: The alkaline solution is selected from one or more of ammonia water, sodium aluminate solution, water glass, and sodium hydroxide solution.

18. A method for preparing the heavy oil type in-situ crystallization catalyst according to any one of claims 1 to 17, characterized in that: The following steps are involved: (1) Preparation of in-situ crystallization products from kaolin microspheres Kaolin is used as raw material, deionized water and silicon-aluminum materials are added, and the mixed slurry is spray-dried to obtain kaolin spray microspheres, which are then calcined, mixed with silicon source, alkaline solution and directing agent for crystallization, and the filter cake is filtered, washed and dried to obtain an in-situ crystallization product; the amount of silicon-aluminum materials added is 1-10% of the mass of kaolin; (2) The in-situ crystallization product is exchanged and calcined to prepare a heavy oil-based in-situ crystallization catalyst The in-situ crystallization product is exchanged and calcined with one or more of ammonium salt, rare earth or phosphorus to obtain a heavy oil type in-situ crystallization catalyst.

19. The method for preparing a heavy oil-based in-situ crystallization catalyst according to claim 18, characterized in that: In step (1), the amount of silicon-aluminum material added is 2-8% of the mass of kaolin.

20. The method for preparing a heavy oil-based in-situ crystallization catalyst according to claim 18, characterized in that: In step (1), a binder is also added when preparing the mixed slurry. The binder is selected from one or more of sodium silicate, silica sol, aluminum sol, and pseudo-boehmite, and the amount added is 2% to 10% of the mass of the kaolin.

21. The method for preparing a heavy oil-based in-situ crystallization catalyst according to claim 18, characterized in that: In step (1), the solid content of the mixed slurry is 30-50 wt %, the particle size of the kaolin spray microspheres is 20-110 μm, the calcination conditions are: 600-1000 ° C for 1-3 hours, and the crystallization conditions are: 90-110 ° C for 18-36 hours.