A catalytic cracking aid for increasing the yield of propylene and a preparation method thereof
By combining silicon-aluminum support material with ZSM-5 molecular sieve, a catalyst with high pore capacity and double pore distribution was prepared, which solved the problem of lower gasoline yield and insufficient heavy oil conversion capacity in the prior art, and achieved high propylene production The rate and good heavy oil conversion capacity have improved the economic benefits of oil refining enterprises.
Patent Information
- Application Number
- CN202111502790.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-09
AI Technical Summary
While existing catalytic cracking additives increase the yield of propylene, they often lead to a decrease in gasoline yield and insufficient conversion capacity of heavy oil, which affects the economic benefits of refining companies.
The silicon-aluminum support material is combined with ZSM-5 molecular sieve to prepare a catalyst with high pore volume, large pore size and good acid distribution. The preheating treatment of acidic aluminum sources and sodium metaaluminate is added to aged. Acidification and alkaline adjustment are then carried out to form a silicon-aluminum material with a biporous distribution for the preparation of catalytic cracking additives.
While increasing the propylene yield, maintain or increase the gasoline yield, enhance the heavy oil conversion capacity, and enhance the economic benefits of oil refining companies.
Smart Images

Figure CN116251618B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of oil refining catalysts, and in particular relates to a propylene-producing catalytic cracking aid and a preparation method thereof. Background Art
[0002] With the construction and commissioning of large-scale domestic refining projects, domestic refining capacity has become oversupplied, the growth rate of demand for refined oil has slowed down, and the demand for basic organic chemical raw materials such as propylene still has a large room for growth. Refining companies will face the need to transform and upgrade from traditional fuel-type refineries to more productive chemical raw materials. Catalytic cracking is the core unit of the refinery. Although a variety of processes and technologies have been developed at home and abroad for the production of more low-carbon olefins, compared with unit modification, the application of catalytic cracking catalysts is still the most economical, quick and effective way to increase the propylene yield of catalytic cracking units.
[0003] The catalytic cracking catalyst can produce more propylene mainly by introducing ZSM-5 or modified ZSM-5 into the catalyst. ZSM-5 molecular sieve has good propylene selectivity in the cracking reaction due to its specific pore structure and acid distribution, as well as good hydrothermal stability. Through the preparation optimization of ZSM-5 molecular sieve, pore modulation and element modification, the performance of the additive in producing more propylene can be improved.
[0004] CN1796497 discloses a catalytic cracking aid for producing more propylene, characterized in that it is composed of 10-65 wt% of modified ZSM-5 molecular sieve, 0-60 wt% of clay, 15-70 wt% of inorganic oxide binder, 0.5-10 wt% of magnesium additive and 0.5-15 wt% of zinc additive, based on the dry catalyst, wherein the modified ZSM-5 molecular sieve is modified by phosphorus. The aid is applied in the catalytic cracking process, and can significantly increase the propylene concentration in the liquefied gas while increasing the yield of catalytic cracking liquefied gas and improving the octane number of gasoline.
[0005] CN107185586 discloses a catalytic cracking aid for producing more propylene and isopentene, and its preparation method and application. The aid contains 15-45% by weight of alkali-modified ZSM-5 molecular sieve. The aid can promote the shape-selective isomerization cracking reaction of gasoline components above C8 in catalytic cracking gasoline, can simultaneously increase the yields of propylene and isopentene, and increase the propylene yield in the liquefied gas increment.
[0006] CN107970981 discloses a catalytic cracking additive for increasing propylene production and a preparation method thereof. The additive comprises, on a dry basis, 10-75 wt% of a phosphorus-containing and metal-loaded MFI structure molecular sieve, 3-40 wt% of a phosphorus-aluminum inorganic binder, 1-30 wt% of other inorganic binders, on a dry basis, 0-60 wt% of a second clay, and 0.5-15 wt% of a metal additive selected from at least one of Group VIII metals and manganese, zinc, and gallium, on an oxide basis. The additive is used in a catalytic cracking process and can effectively improve propylene yield and propylene selectivity.
[0007] CN111760588 discloses a catalytic cracking aid for increasing propylene production, characterized in that the aid contains 10-60 wt% of ZSM-5 molecular sieve, 5-30 wt% of binder, 0.5-5 wt% of phosphorus-containing cationic compound (calculated as P2O5), and 20-80 wt% of clay, based on 100 wt% of dry weight of the aid. The phosphorus-containing cationic compound is used as a modified phosphorus source to significantly improve the phosphorus modification effect. The aid of the present invention is compounded with a catalytic cracking main catalyst to significantly increase the yield of liquefied gas and propylene in the catalytic cracking reaction.
[0008] The above-mentioned patent disclosure mainly modifies ZSM-5 to adjust the pore structure, acid distribution and stability of ZSM-5, thereby improving the propylene yield of the catalytic cracking catalyst or additive. However, the use of the above-mentioned technology to increase propylene production mainly strengthens the selective conversion of gasoline molecules in the ZSM-5 molecular sieve, which often causes a significant decrease in gasoline yield. By optimizing the propylene production-increasing catalyst matrix and Y-type molecular sieve, the conversion of heavy oil and diesel molecular sieves to gasoline is further strengthened, and the gasoline yield is reduced or even not reduced while the catalyst increases propylene production, which is of great significance to improving the economic benefits of oil refining enterprises.
[0009] Moreover, in the heavy oil catalytic cracking process, the use of propylene additives to increase propylene production often reduces the conversion of heavy oil with the addition of propylene additives, resulting in a decrease in the yield of light hydrocarbons cracked on the ZSM-5 molecular sieve, thereby affecting the propylene production increase effect of the additives. By introducing a new carrier into the additive, the impact of the introduction of the additive on the heavy oil conversion capacity of the main catalyst can be reduced.
[0010] CN106179469 introduces a method for preparing a catalyst for increasing propylene production by catalytic cracking. In the invention, ZSM-5 molecular sieve, pseudo-boehmite, clay and water are slurried and then acidified for the first time. After the acidification, water glass is introduced and stirred evenly for the second acidification. After the acidification, alkaline silica sol is added, and after homogenization, spray granulation is performed, washed with water and dried. The invention forms a silica-alumina gel through the acidified pseudo-boehmite and water glass, which has a tetrahedral structure, high hydrothermal stability and medium and large pore distribution. It is suitable for catalytic cracking of heavy oil and can improve the gasoline octane number and propylene yield without reducing or reducing the gasoline yield. However, since the introduced water glass contains a large amount of sodium oxide, it is difficult to reduce the sodium content of the catalyst, which is easy to cause catalyst poisoning, and the use of alkaline silica sol in the system is easy to cause the catalyst strength to be high. Meanwhile, according to the study by Zheng Jinyu et al. in Acta Petrolei Sinica (Petroleum Processing), 2010, 26(6): 846, the volume of mesopores obtained by silicon modification of pseudo-boehmite increased, but the increase was not significant.
[0011] From the above analysis, it can be seen that in order to optimize the propylene selectivity of the co-catalyst, it is usually necessary to modify the shape-selective molecular sieve. However, the traditional propylene co-catalyst prepared by modifying the shape-selective molecular sieve and the main agent often leads to a decrease in the heavy oil conversion capacity of the catalyst. The development of new propylene co-catalysts should reduce or even not reduce the heavy oil conversion capacity of the catalyst while increasing the propylene yield. It is necessary to comprehensively design the carrier and shape-selective molecular sieve of the high-yield propylene co-catalyst.
[0012] CN106179469A introduces a method for preparing a catalyst for increasing propylene production by catalytic cracking. In the invention, ZSM-5 molecular sieve, pseudo-boehmite, clay and water are slurried and then acidified for the first time. After the acidification, water glass is introduced and stirred evenly for the second acidification. After the acidification, alkaline silica sol is added, and after homogenization, spray granulation is performed, washed with water and dried. The invention forms a silica-alumina gel through the acidified pseudo-boehmite and water glass, which has a tetrahedral structure, high hydrothermal stability and medium and large pore distribution. It is suitable for catalytic cracking of heavy oil and can improve the gasoline octane number and propylene yield without reducing or reducing the gasoline yield. However, since the introduced water glass contains a large amount of sodium oxide, it is difficult to reduce the sodium content of the catalyst, which is easy to cause catalyst poisoning, and the use of alkaline silica sol in the system is easy to cause the catalyst strength to be high. Meanwhile, according to the study by Zheng Jinyu et al. in Acta Petrolei Sinica (Petroleum Processing), 2010, 26(6): 846, the volume of mesopores obtained by silicon modification of pseudo-boehmite increased, but the increase was not significant. Summary of the invention
[0013] Based on the above, the main purpose of the present invention is to provide a catalytic cracking aid for producing more propylene and a preparation method thereof. By introducing a silica-alumina carrier material and ZSM-5, a catalyst for producing more propylene is prepared. While producing more propylene, it has a stronger heavy oil conversion ability compared with traditional aids.
[0014] To this end, the present invention provides a catalyst additive for catalytic cracking of high-yield propylene, which comprises 25 to 60 parts of ZSM-5 molecular sieve, 10 to 30 parts of silicon-aluminum material, 10 to 35 parts of clay, 5 to 20 parts of binder, and 1 to 15 parts of P2O5, based on 100 parts of the additive by mass. The silicon-aluminum material has a pseudo-boehmite structure, and its anhydrous chemical expression is (0-0.2) Na2O: (4-30) SiO2: (70-96) Al2O3, and its specific surface area is greater than 500 and not greater than 650m 2 / g, the pore volume is 2.1-2.8mL / g, and the ratio of the pyridine infrared B acid content to the L acid content measured at 200°C is 0.10-0.38.
[0015] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention is preferably that the silicon-aluminum material has a dual pore distribution of 2-40nm and 70-300nm respectively.
[0016] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention is preferably that the silicon-aluminum material is prepared by the following steps:
[0017] (1) preheating the acidic aluminum source and sodium aluminate solution to 45-70° C. respectively, adding them into the reaction kettle in parallel, maintaining the temperature at 45-70° C., stirring the reaction, and the pH value of the reaction is 6-8;
[0018] (2) adding a silicon source at a weight ratio of SiO2:Al2O3=0.05-0.43:1, and adding an alcohol solvent and stirring evenly for primary aging, maintaining the primary aging temperature at 45-70°C and the primary aging pH value at 6-8;
[0019] (3) heating to 80-100° C., adding an alkaline solution to adjust the pH value to 8.5-10.0, and performing secondary aging under stirring to obtain a solid precipitate;
[0020] (4) Filter, wash, exchange and dry the obtained solid precipitate.
[0021] The catalyst aid for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum materials. The preheating first heats the acidic aluminum source and sodium aluminate reaction materials to a certain temperature. This can be achieved in a variety of ways, such as water bath heating, steam heating, and oil bath heating.
[0022] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum materials, wherein the filtering, washing, exchanging and drying of the obtained solid precipitate are conventional technical means in the art, and the exchanging refers to ammonium exchange and / or acid exchange at 60-100° C. after the product is washed. The ammonium exchange is recommended to use the following process conditions: the solid precipitate is exchanged at 60-100° C. according to the weight ratio of precipitate (dry basis): ammonium salt: H2O=1:(0.1-1):(5-10); exchange 1-3 times, each exchange for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.2wt%. The ammonium salt used for the exchange is selected from one or more of ammonium chloride, ammonium nitrate, ammonium carbonate, ammonium sulfate and ammonium bicarbonate. The acid exchange is recommended to use the following process conditions: the solid precipitate is mixed in a weight ratio of precipitate (dry basis): H2O=1:(5-10), then the pH is adjusted to 2.5-3.5 with an acid solution, and the exchange is carried out at 60-100°C; the exchange is performed 1-3 times, each time for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.3wt%. The acid solution used for the exchange is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and citric acid solutions.
[0023] The catalyst aid for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum materials, wherein the drying is a common technique and can be carried out in an oven, or by spray drying or flash drying.
[0024] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing a silicon-aluminum material, wherein the acidic aluminum source is one or more of aluminum nitrate, aluminum sulfate and aluminum chloride.
[0025] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum materials, wherein the concentration of the acidic aluminum source is 50-150 g / L in terms of aluminum oxide, and the concentration of the sodium metaaluminate solution is 20-130 g / L in terms of aluminum oxide.
[0026] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum materials, wherein the silicon source is selected from one or more of water glass, sodium silicate and silicate compounds.
[0027] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing a silicon-aluminum material, wherein preferably, in step (2), the silicon source and the alcohol solvent are added simultaneously, or the silicon source is added first and then the alcohol solvent is added.
[0028] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing a silicon-aluminum material, wherein the acidic aluminum source is based on the weight of aluminum oxide, and the amount of the alcohol solvent added is 1-10 times, preferably 2-5 times, the amount of the acidic aluminum source.
[0029] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum materials, wherein the alcohol solvent is a compound in which hydrogen atoms in saturated aliphatic hydrocarbons and / or alicyclic hydrocarbons are replaced by hydroxyl groups.
[0030] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing a silicon-aluminum material, wherein the alcohol solvent is a C1-C8 monohydric alcohol, a dihydric alcohol or a trihydric alcohol, preferably a C2-C4 alcohol, and further preferably, the alcohol solvent is selected from one or more of ethanol, ethylene glycol, propanol, glycerol, butanol and butanediol.
[0031] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum material, wherein the first aging time is 0.5-3h, and the second aging time is 0.5-3h.
[0032] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing silicon-aluminum material, wherein preferably, the alkaline solution is selected from one or more of ammonia water, sodium metaaluminate solution, water glass, and sodium hydroxide solution.
[0033] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing a silicon-aluminum material, wherein preferably, the exchange includes at least one of ammonium exchange and acid exchange; further preferably, the ammonium exchange is: exchanging the solid precipitate at a weight ratio of 1:0.1-1:5-10 of dry basis precipitate: ammonium salt: H20 at 60-100°C, 1-3 times, each exchange for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.2wt%; further preferably, the ammonium salt is selected from one or more of ammonium chloride, ammonium nitrate, ammonium carbonate, ammonium sulfate, and ammonium bicarbonate.
[0034] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention provides a method for preparing a silicon-aluminum material, wherein preferably, the acid exchange is: mixing the solid precipitate at a weight ratio of precipitate dry basis: H20 of 1:5-10, then adjusting the pH to 2.5-3.5 with an acid solution, and exchanging at 60-100°C; exchanging 1-3 times, each exchange for 0.3-1 hour, until the sodium content in the solid precipitate is less than 0.3wt%; further preferably, the acid solution is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and citric acid solutions.
[0035] The catalyst aid for catalytic cracking of high-yield propylene of the present invention is preferably that the ZSM-5 molecular sieve is at least one of ammonium-type ZSM-5 molecular sieve, hydrogen-type ZSM-5 molecular sieve and modified ZSM-5 molecular sieve. Further preferably, the modified ZSM-5 molecular sieve is a Fe-Ti / ZSM-5 molecular sieve modified by two elements of iron and titanium.
[0036] The catalyst promoter for catalytic cracking of high-yield propylene of the present invention is preferably that the clay is selected from one or more of kaolin, halloysite, montmorillonite, bentonite, sepiolite, attapulgite and rectorite; the P2O5 is derived from a phosphorus-containing compound, and the phosphorus-containing compound is selected from one or more of phosphoric acid, phosphorous acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate; the binder is selected from one or more of aluminum sol, silica sol, silica-alumina sol and silica-alumina gel, and aluminum sol is further preferred.
[0037] To this end, the present invention also provides a method for preparing the above-mentioned high-yield propylene catalytic cracking catalyst additive, comprising the following steps: mixing and slurrying ZSM-5 molecular sieve, silicon-aluminum material, clay, binder and phosphorus source, and then drying and molding; further preferably, the drying is spray molding drying, and its conditions are: the furnace temperature of the spray tower is controlled at 450-550°C, and the spray tail gas temperature is controlled at 200-300°C.
[0038] The method for preparing a catalyst additive for catalytic cracking of high-yield propylene of the present invention preferably further comprises subjecting the dried and shaped catalyst to ion exchange to remove impurity ions therein, and further preferably, the ion exchange is carried out by acid exchange or ammonium exchange, with a pH value of 2.5 to 3.5 and an exchange time of 0.3 to 2 hours.
[0039] The beneficial effects of the present invention are as follows:
[0040] The high-yield propylene catalytic cracking aid provided by the present invention introduces a silicon-aluminum material, which has a high pore volume, a large pore size, a high specific surface area and a good acid distribution, and has good thermal stability and hydrothermal stability. When used in combination with a catalytic cracking main catalyst in heavy oil catalytic cracking, it can promote the conversion of heavy oil macromolecules, produce more light hydrocarbon molecules, and then selective cracking occurs on the ZSM-5 molecular sieve. Through the application of silicon-aluminum materials and ZSM-5, the high-yield propylene catalytic cracking aid prepared by the present invention has higher liquefied gas and propylene yields, lower oil slurry yields and higher gasoline yields. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is the XRD spectrum of the silicon-aluminum and industrial pseudo-boehmite materials prepared in Example 3. Figure 1It shows that the prepared silicon-alumina material has a pseudo-boehmite crystal phase structure, but its crystallinity is lower than that of industrial pseudo-boehmite.
[0042] Figure 2 This is a SEM picture of the silicon-aluminum material prepared in Example 3. The material is composed of stacked nanorods, and two types of pore distributions, mesopores and macropores, can be clearly observed.
[0043] Figure 3 This is the BJH pore distribution curve of the silicon-aluminum material AS-3 prepared in Example 3. Figure 3 It shows that the silicon-aluminum material has a dual pore distribution of 2-40nm and 70-300nm respectively, while the industrial pseudo-boehmite material has only a single pore distribution between 2-4nm, and the pore diameter is 3.4nm. DETAILED DESCRIPTION
[0044] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions, and the unspecified % is weight %.
[0045] Analytical methods
[0046] In each embodiment, the content of Na2O, A12O3 and SiO2 in the product was determined by X-ray fluorescence method (see "Analysis Methods in Petrochemical Industry (RIPP Experimental Methods)", edited by Yang Cuiding et al., Science Press, published in 1990). The specific surface area and pore structure were measured by low-temperature nitrogen adsorption-desorption method, and the pore distribution curve was calculated by BJH method. Scanning electron microscopy (SEM) was characterized by ULTRA-Plus field emission scanning electron microscope of Zeiss, Germany.
[0047] Pyridine adsorption infrared spectroscopy (Py-FTIR) was used to characterize the acid type of the sample using a TENSOR-27 Fourier transform infrared spectrometer produced by Bruker Corporation of the United States. 10 mg of the sample was pressed into a tablet and placed in an in-situ detection cell. The surface was cleaned in a vacuum environment at 350°C for two hours, and then infrared analysis was performed.
[0048] Source of raw materials
[0049] Aluminum chloride, sodium aluminate, aluminum sulfate, aluminum nitrate, propanol, ethanol, ethylene glycol, butanol, butanediol, ammonium nitrate, ammonium sulfate, ammonium chloride, methyl orthosilicate, ethyl orthosilicate, and sodium silicate are analytical reagents and are produced by Sinopharm Chemical Reagent Co., Ltd.
[0050] Sodium silicate, hydrochloric acid, ammonia water, and industrial pseudo-boehmite were provided by PetroChina Lanzhou Petrochemical Catalyst Plant.
[0051] NaY zeolite directing agent, produced by the catalyst plant of Lanzhou Petrochemical Company;
[0052] Kaolin, an industrial product of China Kaolin Corporation, reduced by 20.43%;
[0053] Pseudo-boehmite, produced by Shanxi Aluminum Plant, reduced by 31.5%;
[0054] Aluminum sol, containing 23.7wt% Al2O3, produced by the catalyst plant of Lanzhou Petrochemical Company;
[0055] For the specific preparation method of Fe-Ti / ZSM-5, please refer to Interaction of titanium and iron oxide with ZSM-5 to tune the catalytic cracking of hydrocarbons, Applied Catalysis A: General 375 (2010) 222-229.
[0056] Example 1
[0057] Silicon aluminum material preparation
[0058] Prepare 110g / L aluminum nitrate solution (based on alumina, the same below) and 30g / L sodium aluminate solution, and heat them to 50°C and 55°C respectively. Then, add the aluminum nitrate and sodium aluminate solutions into the reactor in parallel with stirring. Keep the gelling temperature at 52°C during the addition process, and control the addition rate of the two solutions so that the gelling pH value = 6.8. Continue stirring for 45 minutes after the addition is completed, then add water glass according to SiO2:Al2O3=0.29:1. After the addition of water glass, add butanol at 3.5 times the weight of alumina, then continue stirring and aging at 52°C for 1.2 hours, then raise the temperature to 87°C, add water glass to adjust the pH value to 9.2, and stir and age at 87°C for 0.7 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium nitrate: solid precipitate (dry basis): water = 0.25:1:6, and ion exchange is performed at 80°C to remove sodium ions therein. The exchange is repeated once, each time for 0.6h. After each exchange, it is washed and filtered, and then dried at 100°C for 30h to obtain the silicon-aluminum material AS-1 provided by the present invention, and the elemental analysis chemical composition is 0.05Na2O:77.9Al2O3:22.1SiO2.
[0059] Preparation of propylene additives
[0060] 850g water, 240g kaolin (dry basis, the same below), 80g silicon-alumina material AS-1 (dry basis, the same below), 320g Fe-Ti / ZSM-5 molecular sieve (dry basis, the same below), mix and slurry, stir evenly, add 26g phosphoric acid, stir for 45min, then add 759g aluminum sol (solid content, 18.98%, the same below), stir for 2 hours, spray dry, and calcine at 600 degrees for 1.5 hours to obtain the auxiliary agent CAT-1.
[0061] Example 2
[0062] Silicon aluminum material preparation
[0063] Prepare 96g / L aluminum chloride solution and 45g / L sodium aluminate solution, and heat them to 45°C and 48°C respectively. Then, add the aluminum chloride and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 46°C during the feeding process. Control the feeding rate of the two solutions so that the gelling pH value is 6.2. Continue stirring for 35 minutes after the feeding is completed. Then, add sodium silicate solution according to SiO2:Al2O3=0.24:1. After the sodium silicate is added, add propylene glycol at 5.5 times the weight of alumina. Then, continue stirring and aging at 46°C for 2.8 hours, then raise the temperature to 82°C, add sodium hydroxide solution to adjust the pH value to 10.0, and stir and age at 82°C for 1.3 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed at a ratio of solid precipitate (dry basis): water = 1:5, hydrochloric acid is added to adjust the pH to 2.5, and ion exchange is performed at 85°C to remove sodium ions, the exchange is performed for 1.0h, and after the exchange, it is washed and filtered, and then dried at 120°C for 18h to obtain the silicon-aluminum material AS-2 provided by the present invention, and the elemental analysis chemical composition is 0.18Na2O:80.8Al2O3:19.1SiO2.
[0064] Preparation of propylene additives
[0065] 1200g water, 96g kaolin, 136g silicon-alumina material AS-2, 400g Fe-Ti / ZSM-5 molecular sieve are mixed and slurried, and 143g phosphoric acid is added after stirring evenly, and stirred for 80min, followed by adding 421g aluminum sol, stirring for 1.6 hours, spray drying, and calcining at 520 degrees for 2.2 hours to obtain the auxiliary agent CAT-2.
[0066] Example 3
[0067] Silicon aluminum material preparation
[0068] Prepare 120g / L aluminum sulfate solution and 50g / L sodium aluminate solution, and heat them to 60°C and 65°C respectively. Then, add the aluminum sulfate and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 63°C during the feeding process. Control the feeding speed of the two solutions so that the gelling pH value is 7.5. Continue stirring for 15 minutes after the feeding is completed. Then, add methyl orthosilicate solution according to SiO2:Al2O3=0.15:1. After the addition of methyl orthosilicate is completed, add propanol at 3 times the weight of alumina. Then, continue stirring and aging at 63°C for 1.0 hour, then raise the temperature to 95°C, add sodium aluminate solution to adjust the pH value to 8.5, and stir and age at 95°C for 2.0 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium chloride: solid precipitate (dry basis): water = 0.4:1:7, and ion exchange is performed at 90°C to remove sodium ions therein. The exchange is repeated twice, each time for 1.0h. After each exchange, the product is washed and filtered, and then dried at 120°C for 15h to obtain the silicon-aluminum material AS-3 provided by the present invention, and the elemental analysis chemical composition is 0.03Na2O:86.6Al2O3:13.4SiO2.
[0069] Preparation of propylene additives
[0070] 600g water, 100g kaolin, 120g silicon-alumina material AS-3, and 112g Fe-Ti / ZSM-5 molecular sieve are mixed and slurried, and after stirring evenly, 32g phosphoric acid is added and stirred for 30min, followed by adding 253g aluminum sol. After stirring for 1 hour, the mixture is spray-dried and calcined at 500 degrees for 1 hour to obtain the additive CAT-3.
[0071] Example 4
[0072] Silicon aluminum material preparation
[0073] Prepare 145g / L aluminum chloride solution and 95g / L sodium aluminate solution, and heat them to 58°C and 62°C respectively. Then, add the aluminum chloride and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 59°C during the feeding process. Control the feeding speed of the two solutions so that the gelling pH value is 7.7. Continue stirring for 30 minutes after the feeding is completed. Then, add water glass according to SiO2:Al2O3=0.08:1. After the water glass is added, add butanediol at 2.5 times the weight of alumina. Then, continue stirring and aging at 59°C for 2.2 hours, then raise the temperature to 84°C, add ammonia solution to adjust the pH value to 9.7, and stir and age at 84°C for 1.6 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to ammonium sulfate: solid precipitate (dry basis): water = 0.3:1:7, and ion exchange is performed at 87°C to remove sodium ions therein. The exchange is repeated once, each time for 0.9 h. After each exchange, the product is washed and filtered, and then dried at 160°C for 11 h to obtain the silicon-aluminum material AS-4 provided by the present invention, and the elemental analysis chemical composition is 0.04Na2O:92.6Al2O3:7.4SiO2.
[0074] Preparation of propylene additives
[0075] 1500g water, 140g kaolin, 150g silicon-alumina material AS-1, and 550g Fe-Ti / ZSM-5 molecular sieve are mixed and slurried, and after stirring evenly, 160g phosphoric acid is added and stirred for 1 hour, followed by adding 316g aluminum sol. After stirring for 45 minutes, the mixture is spray-dried and calcined at 550 degrees for 1.5 hours to obtain the auxiliary agent CAT-4.
[0076] Example 5
[0077] Silicon aluminum material preparation
[0078] Prepare 75g / L aluminum sulfate solution and 65g / L sodium aluminate solution, and heat them to 68°C and 70°C respectively. Then, add the aluminum sulfate and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 69°C during the feeding process. Control the feeding speed of the two solutions so that the gelling pH value is 7.2. Continue stirring for 25 minutes after the feeding is completed. Then, add tetraethyl orthosilicate solution according to SiO2:Al2O3=0.19:1. After the addition of tetraethyl orthosilicate is completed, add propanol at 7 times the weight of alumina. Then, continue stirring and aging at 69°C for 1.7 hours, then raise the temperature to 92°C, add sodium aluminate solution to adjust the pH value to 9.5, and stir and age at 92°C for 2.4 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to the ratio of ammonium chloride: solid precipitate (dry basis): water = 0.6:1:9, and ion exchange is performed at 93°C to remove sodium ions therein. The exchange is repeated twice, each time for 0.8h. After each exchange, the product is washed and filtered, and then dried at 140°C for 14h to obtain the silicon-aluminum material AS-5 provided by the present invention, and the elemental analysis chemical composition is 0.02Na2O:83.9Al2O3:16.1SiO2.
[0079] Preparation of propylene additives
[0080] 1000g water, 104g kaolin, 200g silicon-alumina material AS-5, 360g Fe-Ti / ZSM-5 molecular sieve are mixed and slurried, and after stirring evenly, 104g phosphoric acid is added and stirred for 50min, followed by adding 379g aluminum sol. After stirring for 1.4 hours, the mixture is spray dried and calcined at 610 degrees for 1.2 hours to obtain the additive CAT-5.
[0081] Example 6
[0082] Silicon aluminum material preparation
[0083] Prepare 55g / L aluminum chloride solution and 35g / L sodium aluminate solution, and heat them to 54°C and 59°C respectively. Then, add the aluminum chloride and sodium aluminate solutions into the reactor in parallel under stirring. Keep the gelling temperature at 56°C during the feeding process. Control the feeding speed of the two solutions so that the gelling pH value is 7.9. Continue stirring for 15 minutes after the feeding is completed. Then, add water glass according to SiO2:Al2O3=0.38:1. After the water glass is added, add ethanol at 9 times the weight of alumina. Then, continue stirring and aging at 56°C for 1.2 hours, then heat to 99°C, add sodium aluminate solution to adjust the pH value to 8.8, and stir and age at 99°C for 2.8 hours. After the obtained product is filtered and washed, the obtained solid precipitate is mixed according to the ratio of ammonium nitrate: solid precipitate (dry basis): water = 0.5:1:10, and ion exchange is performed at 75°C to remove sodium ions therein. The exchange is repeated once, each time for 0.9h. After each exchange, the product is washed and filtered, and then dried at 145°C for 12h to obtain the silicon-aluminum material AS-6 provided by the present invention, and the elemental analysis chemical composition is 0.07Na2O:72.5Al2O3:27.4SiO2.
[0084] Preparation of propylene additives
[0085] 1500g water, 240g kaolin, 300g silicon-alumina material AS-6, 525g Fe-Ti / ZSM-5 molecular sieve are mixed and slurried, and 317g phosphoric acid is added after stirring evenly, and stirred for 70min, followed by adding 1264g aluminum sol. After stirring for 1.2 hours, the mixture is spray dried and calcined at 570 degrees for 2 hours to obtain the additive CAT-6.
[0086] Comparative Example 1
[0087] Industrial pseudo-boehmite was used to replace the silica-alumina material to prepare a comparative catalytic cracking additive. 850g of water, 240g of kaolin, 80g of pseudo-boehmite (dry basis), and 320g of Fe-Ti / ZSM-5 molecular sieve were mixed and slurried, and 26g of phosphoric acid was added after stirring evenly, and stirred for 45 minutes, followed by 759g of aluminum sol. After stirring for 2 hours, the additive was spray-dried and calcined at 600 degrees for 1.5 hours to obtain the additive CAT-7.
[0088] Comparative Example 2
[0089] According to CN201610506039.X, acidified pseudo-boehmite and water glass were used to prepare comparative catalytic cracking aids.
[0090] 600g water, 100g kaolin, 102g pseudo-boehmite (dry basis), 112g Fe-Ti / ZSM-5 molecular sieve, add 20g concentrated hydrochloric acid, stir for 45 minutes, then add 72mL of water glass (silicon dioxide content is 250g / L) to the above slurry, stir for 30 minutes, add 32g of phosphoric acid after stirring evenly, stir for 30min, then add 253g of aluminum sol, stir for 1 hour, spray dry, and calcine at 500 degrees for 1 hour to obtain the additive CAT-8.
[0091] Comparative Example 3
[0092] Prepare silicon-aluminum material according to 201510864343.7.
[0093] Prepare 75g / L aluminum sulfate solution and 65g / L sodium aluminate solution, then add aluminum sulfate and sodium aluminate solution to the reactor in parallel under stirring, control the gelling temperature to 69°C, the pH value of the gelling system = 7.2, and simultaneously mix the ethyl orthosilicate solution with the above gelling slurry in parallel according to SiO2:Al2O3=0.19:1, then heat the slurry to 92°C, stir and age at 92°C for 2.4 hours. After filtering and washing the obtained product, the obtained solid precipitate is mixed according to ammonium chloride: solid precipitate (dry basis): water=0.6:1:9, and ion exchange is performed at 93°C to remove the sodium ions therein, and the exchange is repeated twice, each time for 0.8h, and after each exchange, it is washed and filtered, and then dried at 140°C for 14h to obtain the comparative silicon-aluminum material AS-7.
[0094] Preparation of propylene additives
[0095] 1000g water, 104g kaolin, 200g silicon-alumina material AS-7, 360g Fe-Ti / ZSM-5 molecular sieve are mixed and slurried, and 104g phosphoric acid is added after stirring evenly, and stirred for 50min, followed by adding 379g aluminum sol. After stirring for 1.4 hours, the mixture is spray dried and calcined at 610 degrees for 1.2 hours to obtain the auxiliary agent CAT-9.
[0096] Table 1 provides the pore structure data and pyridine infrared acidity data of samples AS-1 to AS-7 prepared in Examples 1-6 and Comparative Examples 1-3, as well as industrial pseudo-boehmite and comparative tests.
[0097] Table 1 Physicochemical properties of different samples
[0098]
[0099]
[0100] Test Example 1
[0101] Catalyst Evaluation:
[0102] The catalyst reaction performance was evaluated by ACE (an advanced catalyst evaluation) evaluation device produced by Kayser Company of the United States. The raw oil used was Xinjiang vacuum wide fraction wax oil and Xinjiang vacuum residue oil, and the residue blending ratio was 30%. The raw oil properties are shown in Table 2. The catalyst was aged at 800°C and 100% steam for 17 hours before evaluation. The reaction temperature of catalytic cracking was 510°C, and the catalyst-oil mass ratio was 5.0. The LZR-20 catalyst produced by Lanzhou Petrochemical Catalyst Plant was used as the main catalyst. During the evaluation, 6% of the auxiliary agent prepared by the embodiment of the present invention or the comparative example was compounded to evaluate the reaction performance. The evaluation results are shown in Table 3.
[0103] Table 2 Properties of feedstock oil used for catalyst selectivity evaluation
[0104]
[0105]
[0106] Table 3 ACE reaction evaluation results of catalytic cracking additives
[0107]
[0108] It can be seen from Table 3 that the high-yield propylene catalytic cracking additive prepared by the present invention has a better high-yield propylene effect and has a stronger heavy oil conversion ability compared with the comparative additive.
[0109] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. A catalyst promoter for catalytic cracking of high-yield propylene, characterized in that: The additive comprises 25-60 parts of ZSM-5 molecular sieve, 10-30 parts of silicon-aluminum material, 10-35 parts of clay, 5-20 parts of binder and 1-15 parts of P2O5, based on 100 parts of the additive mass composition. The silicon-aluminum material has a pseudo-boehmite structure, and its anhydrous chemical expression is (0-0.2)Na2O: (4-30)SiO2: (70-96)Al2O3, and its specific surface area is greater than 500 m 2 / g, and not more than 650 m 2 / g, the pore volume is 2.1-2.8 mL / g, and the ratio of pyridine infrared B acid content to L acid content measured at 200°C is 0.12-0.
38.
2. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 1, characterized in that: The silicon-aluminum material has a dual pore distribution of 2-40 nm and 70-300 nm respectively.
3. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 1, characterized in that: The silicon-aluminum material is prepared by the following steps: (1) Preheat the acidic aluminum source and sodium aluminate solution to 45-70°C respectively, add them into the reactor in parallel, maintain the temperature at 45-70°C, stir and react, and the pH value of the reaction is 6-8; (2) Add silicon source at a weight ratio of SiO2: Al2O3 = 0.05-0.43:1, and add alcohol solvent and stir evenly for primary aging, maintaining the primary aging temperature at 45-70°C and the primary aging pH value at 6-8; (3) Raising the temperature to 80-100°C, adding an alkaline solution to adjust the pH value to 8.5-10.0, and performing secondary aging under stirring to obtain a solid precipitate; (4) Filter, wash, exchange and dry the obtained solid precipitate.
4. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The acidic aluminum source is one or more of aluminum nitrate, aluminum sulfate and aluminum chloride.
5. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The concentration of the acidic aluminum source is 50-150 g / L in terms of aluminum oxide, and the concentration of the sodium metaaluminate solution is 20-130 g / L in terms of aluminum oxide.
6. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The silicon source is selected from one or more of sodium silicate and silicate compounds.
7. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The silicon source is selected from water glass.
8. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: In step (2), the silicon source and the alcohol solvent are added simultaneously, or the silicon source is added first and then the alcohol solvent.
9. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The acidic aluminum source is based on the weight of aluminum oxide, and the added amount of the alcohol solvent is 1-10 times that of the acidic aluminum source.
10. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 9, characterized in that: The acidic aluminum source is based on the weight of aluminum oxide, and the added amount of the alcohol solvent is 2-5 times that of the acidic aluminum source.
11. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The alcohol solvent is a compound in which hydrogen atoms in saturated aliphatic hydrocarbons and / or alicyclic hydrocarbons are replaced by hydroxyl groups.
12. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 11, characterized in that: The alcohol solvent is a C1-C8 monohydric alcohol, dihydric alcohol or trihydric alcohol.
13. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 11, characterized in that: The alcohol solvent is a C2-C4 alcohol.
14. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 11, characterized in that: The alcohol solvent is selected from one or more of ethanol, ethylene glycol, propanol, glycerol, butanol and butanediol.
15. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The time of the first aging is 0.5-3 h, and the time of the second aging is 0.5-3 h.
16. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 3, characterized in that: The alkaline solution is selected from one or more of ammonia water, sodium aluminate solution, water glass, and sodium hydroxide solution.
17. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 1, characterized in that: The ZSM-5 molecular sieve is at least one selected from ammonium ZSM-5 molecular sieve, hydrogen ZSM-5 molecular sieve and modified ZSM-5 molecular sieve.
18. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 17, characterized in that: The modified ZSM-5 molecular sieve is a Fe-Ti / ZSM-5 molecular sieve modified by two elements, iron and titanium.
19. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 1, characterized in that: The clay is selected from one or more of kaolin, halloysite, montmorillonite, bentonite, sepiolite, attapulgite, and rectorite; the P2O5 is derived from a phosphorus-containing compound, and the phosphorus-containing compound is selected from one or more of phosphoric acid, phosphorous acid, diammonium hydrogen phosphate, diammonium hydrogen phosphate, and ammonium phosphate; the binder is selected from one or more of aluminum sol, silica sol, silica-alumina sol, and silica-alumina gel.
20. The catalyst promoter for catalytic cracking of high-yield propylene according to claim 19, characterized in that: The binder is aluminum sol.
21. A method for preparing a catalyst promoter for catalytic cracking of high-yield propylene according to claim 1, characterized in that: The method comprises the following steps: mixing and slurrying ZSM-5 molecular sieve, silicon-aluminum material, clay, binder and phosphorus source, and then drying and forming.
22. The preparation method according to claim 21, characterized in that: The method also includes subjecting the dried and shaped catalyst to acid exchange or ammonium exchange treatment.