Method for manufacturing hollow sphere

Precursors are prepared by mixing fly ash, expansion agent and liquid resin, and coated with silicon-containing compounds and heat-treated to form hollow spheres, which solves the problems of high cost and poor forming properties of hollow spheres, and achieves low cost and high forming The manufacturing of hollow spheres has enhanced its application.

CN116253519BActive Publication Date: 2024-12-03METAL INDS RES & DEV CENT
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111458671.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-02
Publication Date
2024-12-03
Estimated Expiration
2041-12-02

AI Technical Summary

Technical Problem

The existing hollow sphere manufacturing methods have high material costs, the forming properties, pressure and temperature resistance need to be improved, and the process is complex, which cannot meet the needs of special fields.

Method used

The precursor is prepared by mixed fly ash, expansion agent and liquid resin, and then coated with silicon-containing compounds and heat treatment is carried out to form a silicon-containing shell layer and hollow sphere, reducing material costs and simplifying the process.

Benefits of technology

It improves the formingability and yield of hollow spheres, reduces process energy consumption, forms low-cost green materials, and enhances the application of hollow spheres.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116253519B_ABST
    Figure CN116253519B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a hollow sphere and the hollow sphere thereof, which reduces material cost by using fly ash and uses a simpler and lower energy consumption process operation, so that the hollow sphere has a higher forming rate, thereby increasing the applicability of the hollow sphere.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a hollow sphere and the hollow sphere, in particular to a method for manufacturing a hollow sphere with high formability and the hollow sphere. Background Art

[0002] Hollow sphere materials have the functions of lubrication, low density, light weight, heat insulation and sound insulation, so they are widely used. The application of hollow spheres in the mid-to-high-end market includes oil well exploration, solid floating materials in marine technology, interior panels in the aerospace and construction industries. In addition, special needs in recent years (such as: hydrogen storage materials, lithium battery negative electrode materials, electromagnetic wave shielding materials and microwave signal absorption materials, etc.) are also one of the key points of future hollow sphere material research and development. For example, the hollow glass balls developed by 3M's advanced materials department enable European urban buildings to reduce energy use through heat insulation, thereby reducing carbon emissions. In terms of the market, about 1,200 tons of glass hollow spheres are used each year, which are mainly used in building materials, but due to the future offshore wind power construction and operation and maintenance and other related marine technology development needs, it is expected to further drive the large-scale application demand for hollow sphere materials.

[0003] Conventional hollow spheres are usually hollow glass microspheres whose main component is borosilicate, which are manufactured by methods such as solid powder method, spray granulation method, dry gel method or droplet method, etc. However, the material cost of the conventional method is relatively high and cannot meet the requirements of use in special fields.

[0004] There are many related previous cases about hollow spheres. For example, Chinese patent publication No. CN 102320743 discloses a high-strength hollow glass microsphere made of aluminum silicate and a preparation method thereof, which comprises the following steps: melting the mixed raw materials in a crucible; then quenching with water and drying; then crushing and grinding by air flow to separate powders of a specific particle size; finally, feeding the powders into a spheroidizing furnace to obtain hollow glass microspheres, which can be used in high temperature and / or high pressure environments, thereby improving the applicability of the hollow glass microspheres.

[0005] In addition, Chinese patent publication number CN 105392742 discloses a glass microbubble, a crude product and a preparation method thereof, which is prepared by adding metal oxide powder and an expansion agent into a binder to prepare a ceramic slurry, and then atomizing and granulating the mixture with a spray dryer to obtain a precursor powder; and then forming a hollow sphere by flame combustion to obtain a glass hollow sphere.

[0006] Furthermore, U.S. Patent No. US 7878026 discloses a synthetic hollow sphere, which is formed by aluminosilicate and a binder to form a precursor, and then forms solid or hollow microspheres through composition and heating temperature control to replace natural fly ash hollow microspheres. It can be suitable for filling into cement compositions, has better chemical durability, and can also reduce material costs and improve productivity.

[0007] However, the above conventional methods all use glass as the main component, and the compressive strength, temperature resistance and environmental tolerance of the hollow sphere after forming still have room for improvement. In addition, although the additional addition of multiple oxides can improve the applicability of the product, it also increases the material cost and makes the process complicated, thereby increasing the difficulty of forming the hollow sphere.

[0008] In view of this, there is an urgent need to provide a hollow sphere and a manufacturing method thereof to reduce material costs and improve the formability of the hollow sphere, thereby increasing the applicability of the hollow sphere. Summary of the invention

[0009] One aspect of the present invention is to provide a method for manufacturing a hollow sphere, which can improve the formability and yield of the hollow sphere and reduce the energy consumption of the hollow sphere manufacturing process.

[0010] Another aspect of the present invention is to provide a hollow sphere, which is a low-cost green material.

[0011] According to one aspect of the present invention, a method for manufacturing a hollow sphere is provided. The method comprises mixing fly ash, an expansion agent and a liquid resin to obtain a precursor. The amount ratio of the expansion agent to the fly ash is 0.2 to 3. Then, a silicon-containing compound is sprayed on the surface of the precursor so that the silicon-containing compound covers the precursor to obtain a modified precursor. Then, the modified precursor is heat-treated so that the modified precursor produces a thermochemical reaction to release gas, and a silicon-containing shell layer is formed on the periphery of the modified precursor, and the gas is covered by the silicon-containing shell layer to form a hollow sphere.

[0012] According to an embodiment of the present invention, the temperature of the heat treatment is 750°C to 1400°C.

[0013] According to an embodiment of the present invention, the above-mentioned operation of spraying the silicon-containing compound further includes baking the precursor and the silicon-containing compound. The baking operation is performed at a temperature of 80° C. to 150° C. for 5 minutes to 15 minutes.

[0014] According to an embodiment of the present invention, the expansion agent includes boric acid, borax, urea, water glass and / or a combination thereof.

[0015] According to an embodiment of the present invention, the silicon-containing compound includes silicone resin, sodium silicate, sodium metasilicate and / or a combination thereof.

[0016] According to an embodiment of the present invention, based on the total weight of the expansion agent and the fly ash being 100wt%, the added amount of the liquid resin is 8wt% to 12wt%.

[0017] According to an embodiment of the present invention, the liquid resin includes phenolic resin and / or high-density polyethylene.

[0018] According to another aspect of the present invention, a hollow sphere is provided, which is prepared by the method provided by the above aspect. The hollow sphere comprises 60wt% to 70wt% of silicon dioxide, 10wt% to 15wt% of aluminum oxide, 5wt% to 10wt% of sodium oxide, 5wt% to 10wt% of iron oxide, 4wt% to 5wt% of calcium oxide, 1wt% to 2wt% of magnesium oxide and other unavoidable components.

[0019] According to an embodiment of the present invention, the hollow sphere has a core-shell structure, and the shell thickness of the hollow sphere is 1 μm to 50 μm.

[0020] According to an embodiment of the present invention, the average particle size of the hollow spheres is 30 μm to 1 mm.

[0021] The hollow sphere manufacturing method and the hollow sphere of the present invention reduce material costs by using fly ash and use a simpler and less energy-consuming process operation, so that the hollow sphere has a higher forming rate, thereby increasing the applicability of the hollow sphere. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present disclosure is better understood by reading the following detailed description in conjunction with the accompanying drawings. It should be noted that, as is standard practice in the industry, many features are not drawn to scale. In fact, for the sake of clarity of discussion, the dimensions of many features may be arbitrarily scaled.

[0023] Figure 1 is a flow chart illustrating a method for manufacturing a hollow sphere according to some embodiments of the present invention;

[0024] FIG. 2A to FIG. 2C are scanning electron microscopic images of hollow spheres according to some embodiments of the present invention.

[0025]

Explanation of symbols

[0026] 100: Method

[0027] 110,120,130: Operation DETAILED DESCRIPTION

[0028] As used in this disclosure, “around,” “about,” “approximately,” or “substantially” generally means within 20 percent, or within 10 percent, or within 5 percent of the stated value or range.

[0029] As described above, the present invention provides a hollow sphere and a method for manufacturing the same, which reduces material costs by using fly ash and uses a simpler and less energy-consuming process operation, so that the hollow sphere has a higher forming rate, thereby increasing the applicability of the hollow sphere.

[0030] See also Figure 1 , which is a flow chart of a method 100 for manufacturing a hollow sphere according to some embodiments of the present invention. First, operation 110 is performed to mix fly ash, an expander and a liquid resin to obtain a precursor. In some embodiments, this step can first uniformly mix the fly ash and the expander, directly granulate, and then spray the liquid resin on the outer surface of the aforementioned mixture, by directly adsorbing an appropriate amount of liquid resin on the mixture of fly ash and the expander to increase the overall solid content of the precursor, and can reduce the subsequent reprocessing procedures to quickly achieve granulation. In other embodiments, fly ash, an expander and a liquid resin can also be mixed by dry mixing to reduce the amount of liquid resin (compared to the amount of the conventional method) to achieve the effect of rapid solidification granulation. Preferably, based on the total weight of the expander and fly ash mixed as 100wt%, the amount of liquid resin added can be about 8wt% to about 12wt%. In some embodiments, the amount ratio of the expander and fly ash is 0.2 to 3, and the preferred amount ratio is 3. This ensures that the precursor formed by granulation has an appropriate particle size, can form a hollow sphere after the subsequent process, and makes the hollow sphere have a better forming rate. Furthermore, the amount of expansion agent is small, which helps to improve the density of the hollow sphere. If too much expansion agent is added (for example, the aforementioned amount ratio is greater than 3), the hollow sphere may explode due to excessive expansion after subsequent processing; on the contrary, if the amount of expansion agent is too small (for example, the aforementioned amount ratio is less than 0.2), an effective expansion effect cannot be achieved.

[0031] Generally speaking, fly ash refers to fine particles flying in the air. The fly ash used in the present invention is not particularly limited, and may be, for example, industrial fly ash produced by burning coal in an industrial process. In some embodiments, the fly ash may contain silicon dioxide, aluminum oxide, iron oxide and other unavoidable components. In some embodiments, the particle size of the fly ash is 1 μm to 15 μm. The particle size of the fly ash will affect the heat treatment temperature in the subsequent process, so when the fly ash particle size is within the aforementioned range, the subsequent heat treatment temperature can be effectively controlled within an appropriate range.

[0032] In some embodiments, the expansion agent includes boric acid, borax, urea, a water-containing compound [such as water glass (sodium silicate)] and / or a combination thereof. In some embodiments, the liquid resin may be a thermosetting or thermoplastic resin, such as a phenolic resin or high-density polyethylene, preferably a curable phenolic resin, so as to be cured by a subsequent heat treatment operation. In some embodiments, the liquid resin may be prepared by mixing an equal proportion (such as weight ratio) of a phenolic resin and a solvent (such as water, alcohol, etc.).

[0033] Next, operation 120 is performed to spray a silicon-containing compound on the surface of the above-mentioned precursor so that the silicon-containing compound covers the precursor to obtain a modified precursor. In some embodiments, the silicon-containing compound comprises silicone resin, sodium silicate, sodium metasilicate and / or a combination thereof. In some embodiments, operation 120 may selectively include a low-temperature baking operation on the precursor and the silicon-containing compound, for example, spraying the silicon-containing compound while baking to accelerate the drying and forming of the modified precursor. In some embodiments, the low-temperature baking operation is performed at a temperature of 80°C to 150°C for 5 minutes to 15 minutes. The resulting modified precursor is a granular sphere having a silicon-containing compound coated on the surface of the precursor. In some embodiments, based on the precursor being 100wt%, the amount of silicon-containing compound added may be 2wt% to 5wt%. The precursor is coated with a silicon-containing compound to coat the unstable components of the fly ash during the subsequent high-temperature heat treatment to generate gases. The thickness of the desired hollow sphere and the composition ratio of the precursor can be adjusted by the amount of the silicon-containing compound sprayed, thereby obtaining a hollow sphere with specific properties.

[0034] Then, operation 130 is performed to heat-treat the modified precursor to obtain a hollow sphere. The heat-treating operation utilizes high temperature to heat the modified precursor to generate a reaction and release gas. In addition, the silicon-containing compound coated on the surface of the modified precursor can be transformed into a fluid silicon-containing shell layer because the temperature is higher than its glass transition temperature, and the released gas is encapsulated to form a hollow structure of the sphere.

[0035] In some embodiments, the temperature of the heat treatment is 750°C to 1400°C, preferably 750°C to 1100°C, and more preferably 800°C to 1050°C. If the temperature of the heat treatment is lower than 750°C, the expansion agent cannot react effectively, and the gas is released to form the hollow sphere; but if the temperature of the heat treatment is higher than 1400°C, there is no obvious gain effect, and only energy is wasted. In some embodiments, the high-temperature heat treatment is performed for no more than 10 seconds, preferably no more than 5 seconds. The high-temperature heat treatment time should not be too long to avoid directly burning the hollow sphere. In some embodiments, the temperature can be selectively rapidly cooled after the high-temperature heat treatment to obtain a hollow sphere with a lower density by rapidly heating and cooling the temperature.

[0036] The hollow sphere obtained by the above method has a core-shell structure, and the core-shell structure is a silicon-containing shell layer, especially a ceramic shell layer. In some embodiments, the shell thickness of the hollow sphere is 1μm to 50μm. The shell thickness will affect the structural strength and density of the hollow sphere. Generally speaking, the smaller the shell thickness, the smaller the structural strength and the smaller the density; the larger the shell thickness, the greater the structural strength and the greater the density. Therefore, the present invention can adjust the shell thickness within the aforementioned range according to application requirements. In some embodiments, the average particle size of the hollow sphere is 30μm to 1mm, preferably 50μm to 500μm, and more preferably 50μm to 100μm. Generally, the process cost of hollow spheres with smaller particle sizes is higher, and conversely, the process cost of hollow spheres with larger particle sizes is also lower. Furthermore, the particle size of the hollow sphere must also be adjusted according to application requirements.

[0037] In some embodiments, based on 100wt% of the hollow sphere, the composition of the hollow sphere includes 60wt% to 70wt% of silicon dioxide, 10wt% to 15wt% of aluminum oxide, 5wt% to 10wt% of sodium oxide, 5wt% to 10wt% of iron oxide, 4wt% to 5wt% of calcium oxide, and 1wt% to 2wt% of magnesium oxide and other unavoidable components. The hollow sphere is a green material formed through fly ash and has considerable strength and appropriate density. Furthermore, when the hollow sphere is used as a buoyancy material, it can present better pressure resistance and buoyancy.

[0038] Several embodiments are used below to illustrate the application of the present invention, but they are not used to limit the present invention. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention.

[0039] Example

[0040] The embodiment uses industrial fly ash from Formosa Plastics Thermal Power Plant, which contains more than 50wt% of silicon dioxide, 22wt% to 30wt% of aluminum oxide, 7wt% to 10wt% of iron oxide, 3wt% to 5wt% of calcium oxide and 2wt% to 4wt% of magnesium oxide and other unavoidable components based on 100wt% of industrial fly ash. The average particle size of this industrial fly ash is 5μm to 8μm. First, the aforementioned industrial fly ash, borax and phenolic resin solution are dry-mixed to form a granular precursor containing fly ash. The mixing ratio of industrial fly ash and expansion agent described in this embodiment is 3:1. In addition, the phenolic resin solution described in this embodiment is diluted with alcohol and phenolic resin in a weight percentage ratio of 1:1.

[0041] Next, the granular precursor is baked at 80°C for 10 minutes, and the silicone resin is sprayed repeatedly during the process so that the silicone resin evenly covers the outer surface of the granular precursor to obtain a modified granular precursor. Then, the modified granular precursor is placed in a high temperature environment of 750°C for 5 seconds for heat treatment, and expands through a thermochemical reaction to obtain a hollow sphere.

[0042] The hollow spheres prepared above were analyzed to contain 62.46 wt% silicon dioxide, 12.17 wt% aluminum oxide, 8.10 wt% sodium oxide, 7.86 wt% iron oxide, 4.29 wt% calcium oxide, 1.3 wt% magnesium oxide and other unavoidable ingredients. FIG. 2A to FIG. 2C As shown, the hollow spheres prepared in the example were observed using a scanning electron microscope. Figure 2A and Figure 2B It can be seen that the hollow sphere comprises a core-shell structure with a silicon-containing shell layer. FIG. 2A to FIG. 2C The average particle sizes of the hollow spheres are about 62 μm, 100 μm and 128 μm, respectively. Figure 2A The thickness of the silicon-containing shell layer is about 1.3 μm to 1.5 μm. Figure 2B The thickness of the silicon-containing shell layer is about 3 μm.

[0043] From the above embodiments, it can be seen that the hollow spheres produced by the hollow sphere manufacturing method of the present invention can have the expected shell thickness and particle size, and can present better strength and buoyancy characteristics. Furthermore, the aforementioned hollow spheres have good formability, and can be formed into hollow spheres with different shell thicknesses and different particle sizes to be suitable for products with different application ends, so they have better commercial properties.

[0044] According to the above embodiments, the manufacturing method of the hollow sphere and the hollow sphere provided by the present invention reduce material costs by using fly ash, and use a simpler and lower energy consumption process operation, so that the hollow sphere has a higher forming rate, thereby increasing the applicability of the hollow sphere.

[0045] Although the present invention has been disclosed as above with several embodiments, they are not intended to limit the present invention. Anyone with ordinary knowledge in the technical field to which the present invention belongs can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the attached claims.

Claims

1. A method for manufacturing a hollow sphere, characterized in that: Include: Mixing fly ash, an expansion agent and a liquid resin to obtain a precursor, wherein a ratio of the expansion agent to the fly ash is 0.2 to 3; Spraying a silicon-containing compound onto a surface of the precursor so that the silicon-containing compound covers the precursor to obtain a modified precursor; as well as The modified precursor is subjected to a heat treatment to cause a thermochemical reaction to release a gas, and a silicon-containing shell is formed on the outer periphery of the modified precursor. The gas is encapsulated by the silicon-containing shell to form the hollow sphere, wherein a temperature of the heat treatment is 750° C. to 1400° C.

2. The method for manufacturing a hollow sphere according to claim 1, characterized in that: The operation of spraying the silicon-containing compound further comprises: A baking operation is performed on the precursor and the silicon-containing compound, wherein the baking operation is performed at a temperature of 80° C. to 150° C. for 5 minutes to 15 minutes.

3. The method for manufacturing a hollow sphere according to claim 1, characterized in that: The expansion agent comprises boric acid, borax, urea, water glass and / or a combination thereof.

4. The method for manufacturing a hollow sphere according to claim 1, characterized in that: The silicon-containing compound includes silicone resin, sodium silicate, sodium metasilicate and / or a combination thereof.

5. The method for manufacturing a hollow sphere according to claim 1, characterized in that: Based on a total weight of the expansion agent and the fly ash being 100 wt %, an addition amount of the liquid resin is 8 wt % to 12 wt %.

6. The method for manufacturing a hollow sphere according to claim 1, characterized in that: The liquid resin is phenolic resin and / or high-density polyethylene.

7. The method for manufacturing a hollow sphere according to claim 1, characterized in that: The hollow sphere contains 60wt% to 70wt% of silicon dioxide, 10wt% to 15wt% of aluminum oxide, 5wt% to 10wt% of sodium oxide, 5wt% to 10wt% of iron oxide, 4wt% to 5wt% of calcium oxide, 1wt% to 2wt% of magnesium oxide and other inevitable ingredients.

8. The method for manufacturing a hollow sphere according to claim 1, characterized in that: The hollow sphere has a core-shell structure, and a shell thickness of the hollow sphere is 1 μm to 50 μm.

9. The method for manufacturing a hollow sphere according to claim 1, characterized in that: An average particle size of the hollow sphere is 30 μm to 1 mm.

Citation Information

Patent Citations

  • Synthetic microspheres and methods of making same

    US7878026B2

  • Hollow Microspheres

    CN102811965A