A preparation method of lithium niobate thin film superlattice waveguide and comb electrode

By etching first and then polarizing on the lithium niobate film, and using comb electrodes to form a rectangular domain structure, the problems of high waveguide loss and poor domain structure quality are solved, and efficient preparation of lithium niobate film superlattice waveguides is achieved to meet industrial performance need.

CN116256841BActive Publication Date: 2024-11-26NANJING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211604389.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-26
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

In the prior art, in the preparation process of lithium niobate thin film superlattice waveguides, the corrosion liquid selectivity problem caused by first polarization and etching leads to high waveguide losses and poor domain structure quality, and the domain of the etching and then polarization process The structural quality is poor and it is difficult to meet industrial performance needs.

Method used

Using the process of etching first and then polarization, a comb-shaped electrode is prepared on a lithium niobate film, and polarized using the electrode structure of the tip and fingers and a flat finger to form a rectangular domain structure, reducing waveguide losses and improving the quality of the domain structure.

Benefits of technology

The waveguide loss reduction and the domain structure quality are improved, and the normalization efficiency reaches nearly 2000% W-1·cm-2, meeting industrial performance needs, and improving the flexibility of the process flow and parameter control accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116256841B_ABST
    Figure CN116256841B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and a comb-shaped electrode of a lithium niobate thin film superlattice waveguide, and the preparation method comprises: etching to obtain a lithium niobate thin film waveguide and a comb-shaped electrode structure; the comb finger part of the comb-shaped electrode is arranged periodically, the comb finger is perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers; the electrode on the side with the pointed fingers is connected to the positive pole of the circuit, and the electrode on the other side is grounded, and an electric field is applied to cause the lithium niobate in the area covered by the metal electrode to undergo domain flipping; the electrode is removed to obtain a domain flipping structure in the waveguide area, and further obtain a lithium niobate thin film superlattice waveguide. The application greatly reduces the waveguide loss caused by the selective corrosion of positive and negative polarity domains during the cleaning process in the process of polarizing first and then etching the waveguide, and at the same time, the comb-shaped electrode structure can polarize a rectangular domain with a very thin domain wall, improve the quality of the domain, and facilitate the connection of subsequent processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor integrated optoelectronic devices, and in particular to a preparation method of a lithium niobate thin film superlattice waveguide and a comb-shaped electrode. Background Art

[0002] Integrated optics was first proposed by Bell Labs in the United States in 1969. It has gone through a process of starting, developing and becoming increasingly mature, and is now widely used in many fields. The most basic and important component in integrated optics is the optical waveguide. The optical waveguide mainly uses the principle of total reflection of light to confine the light to propagate in a medium of the wavelength order. Waveguide loss is an important factor in measuring the performance of the optical waveguide. Lithium niobate is currently the most commonly used optical waveguide medium. The most commonly used process in nonlinear optics on lithium niobate films is the second-order nonlinear process. Due to the high second-order nonlinear coefficient of LN itself and the strong binding effect brought by the LNOI system, the intensity of the nonlinear process in the LNOI system is higher. In the LNOI system, due to the small size of the device, the birefringence matching method is no longer applicable, and the quasi-phase matching method becomes the mainstream. Quasi-phase matching depends on periodic domain inversion, that is, the preparation of waveguide superlattice.

[0003] At present, the common technology for lithium niobate thin film is to first polarize the lithium niobate thin film waveguide, then remove the electrode and etch the waveguide on its surface. During the cleaning step after etching of the polarized sample, the surface of the waveguide area with periodic domain inversion is wrinkled due to the selective etching of the corrosive solution, which increases the loss of the waveguide. The technicians in the industry have also tried to prepare lithium niobate thin film superlattice waveguide by etching first and then polarizing, but the quality of the obtained lithium niobate thin film superlattice waveguide is significantly lower than that of the lithium niobate thin film superlattice waveguide prepared by polarizing first and then etching. Therefore, the industry does not recognize the process of etching first and then polarizing to prepare lithium niobate thin film superlattice waveguide.

[0004] The paper Locally periodically poled LNOIridge waveguide for second harmonic generation [Invited] [J] discloses an etch-before-poling process for preparing lithium niobate thin film superlattice waveguides. The etch-before-poling process is used to reduce the loss of the waveguide with periodic domain inversion. However, this etch-before-poling process polarizes a triangular domain structure in the lithium niobate waveguide. The quality of the domain structure is poor, which greatly reduces the theoretical and experimental efficiency of the waveguide structure.

[0005] How to prepare a lithium niobate thin film superlattice waveguide with low waveguide loss and high domain structure quality through the process of etching first and then polarizing is a technical problem that needs to be solved urgently. Summary of the invention

[0006] The solution of the present application is based on the above ideas and provides a method for preparing a lithium niobate thin film superlattice waveguide and a comb electrode constructed during the preparation process. It uses a method of first etching the waveguide and then polarizing it, and polarizes a rectangular domain structure through the comb electrode, thereby solving the problem of high waveguide loss caused by the process.

[0007] On the one hand, the present application provides a method for preparing a lithium niobate thin film superlattice waveguide, comprising the following steps:

[0008] 1) preparing an overlay mark, and using a photolithography method to prepare a waveguide shape profile on the surface of an x-cut lithium niobate film according to the overlay mark;

[0009] 2) etching a waveguide structure on the surface of the x-cut lithium niobate film, removing the electron beam glue, and obtaining a lithium niobate film waveguide;

[0010] 3) According to the overlay marks, a comb-shaped electrode shape profile is prepared on the surface of the x-cut lithium niobate film by photolithography, and a metal electrode is plated on the photolithographic comb-shaped electrode shape profile to obtain an intermediate sample; wherein the comb fingers of the comb-shaped electrode are arranged periodically, the comb fingers are perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers;

[0011] 4) removing the photoresist to obtain a polarized electrode structure;

[0012] 5) Connect the electrode on one side of the comb finger to the positive electrode of the circuit, and the electrode on the other side is grounded, and an electric field is applied to cause the lithium niobate in the area covered by the metal electrode to undergo domain reversal;

[0013] 6) Using dilute hydrochloric acid to remove the electrodes, obtaining a domain flipping structure in the waveguide region;

[0014] 7) Polishing the end face of the waveguide to obtain a lithium niobate thin film superlattice waveguide.

[0015] Furthermore, the preparation of the overlay mark comprises:

[0016] Using photolithography to prepare an overlay mark photoresist pattern on a sample wafer;

[0017] Plating a layer of metal on the photolithographic sample, wherein the thickness of the metal is 30 to 300 nm;

[0018] Use acetone or nmp solution to remove the photoresist to obtain the overlay mark.

[0019] Furthermore, the width of the comb-shaped electrodes is 1 / 4 to 1 / 3 of the period length.

[0020] Furthermore, the comb-shaped electrode is 25um long, the tip length of the pointed finger is 5um, the period length is 3-4um, the electrode width is 0.8-1um, and the distance between the positive and negative electrodes is 6um.

[0021] Furthermore, the metal electrode is one of aluminum, nickel, chromium or titanium.

[0022] Furthermore, the voltage of the applied electric field is 100-400V.

[0023] Further, the above-mentioned method comprises preparing a comb-shaped electrode profile on the surface of the x-cut lithium niobate film by photolithography according to the overlay mark, and plating a layer of metal electrode on the photolithographic comb-shaped electrode profile to obtain an intermediate sample, which comprises:

[0024] According to the overlay marks, the comb finger part outline of the comb-shaped electrode shape outline is prepared on the surface of the x-cut lithium niobate film by using a photolithography method, wherein the comb fingers are perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers;

[0025] A layer of metal electrode is plated on the contour of the photoetched comb finger portion;

[0026] The photoresist is removed to obtain periodically arranged comb-finger electrodes;

[0027] According to the overlay marks, a flat plate portion outline of a comb-shaped electrode is prepared on the surface of the x-cut lithium niobate film by using a photolithography method, wherein the flat plate portion outline covers a portion of the comb-shaped finger electrode;

[0028] A layer of metal electrode is plated on the contour of the photolithographic flat plate to obtain an intermediate sample.

[0029] Furthermore, the method for removing the electron beam glue is to use RCA solution for corrosion removal, and the formula of the RCA solution is ammonia water: hydrogen peroxide: water = 1:2:7.

[0030] Furthermore, the photolithography method is electron beam lithography, ultraviolet lithography or a combination of electron beam lithography and ultraviolet lithography; the method for removing the photoresist is to use acetone or N-methylpyrrolidone solution to corrode and remove the photoresist.

[0031] On the other hand, the present application also provides a comb-shaped electrode, which is used to prepare the above-mentioned lithium niobate thin film superlattice waveguide, and is obtained by preparing a comb-shaped electrode shape contour on the surface of an x-cut lithium niobate thin film by photolithography, and plating a layer of metal electrode on the photolithographic comb-shaped electrode shape contour; the comb finger part of the comb-shaped electrode is arranged periodically, the comb fingers are perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers.

[0032] The present invention first prepares a lithium niobate waveguide structure on a lithium niobate film, and then uses a specially designed comb electrode structure to polarize the waveguide region to polarize a high-quality rectangular domain structure in the waveguide region, and verifies the feasibility of the experiment through nonlinear optical testing. Compared with the prior art, the preparation method of first etching a waveguide on a lithium niobate film and then polarizing the waveguide region can place the polarization after the waveguide and related process steps, thereby improving the flexibility of the related process flow. Due to the experimental error, technicians can test the specific parameters of the waveguide after the previous process, and then make targeted designs to accurately control the polarization period. At the same time, compared with the process of first etching and then polarizing to polarize a triangular domain structure, the normalized efficiency of the lithium niobate film superlattice waveguide prepared by the present invention can reach nearly 2000% W. -1 cm -2 , which can meet the performance requirements of industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The following is a brief description of the contents expressed in the drawings of the specification:

[0034] Figure 1 Schematic diagram of the structure of the comb-shaped polarized electrode in the present invention;

[0035] Figure 2 It is a schematic diagram of the process of preparing a lithium niobate thin film superlattice waveguide in an embodiment of the present invention;

[0036] Figure 3 This is a confocal image of the lithium niobate thin film superlattice waveguide prepared in Example 1 of the present invention;

[0037] Figure 4 This is a confocal image of the lithium niobate thin film superlattice waveguide prepared in Example 2 of the present invention;

[0038] Figure 5 This is a graph showing the normalized frequency doubling efficiency results in optical testing of the lithium niobate thin film superlattice waveguide prepared in Example 1 of the present invention;

[0039] Figure 6 This is a diagram showing the light intensity results of the optical test of the lithium niobate thin film superlattice waveguide prepared in Example 1 of the present invention;

[0040] Figure 7 This is a characterization image of the side wall of the lithium niobate waveguide prepared in the comparative example of the present invention under an electron microscope;

[0041] Figure 8 This is a confocal image of the polarization region of a lithium niobate waveguide prepared as a comparative example of the present invention. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] In order to reduce the waveguide loss caused by the selective corrosion of positive and negative polarity domains during the cleaning process when the waveguide is first polarized and then etched, the present invention provides another processing sequence, that is, etching the waveguide first and then polarizing the waveguide, which is helpful for connecting other processes. At the same time, in order to improve the quality of the domain in the lithium niobate superlattice waveguide, the present invention provides a rectangular domain with very thin domain walls.

[0044] In order to polarize this rectangular domain, the present invention designs an electrode structure of pointed fingers to flat fingers, such as Figure 1 As shown, the electrode with the tip structure is connected to the positive electrode, and the electrode width is 1 / 3 to 1 / 4 of the period. If the specific fine structure of the waveguide is confirmed by electron microscopy or other methods before polarization, the structure of a specific wavelength can be simulated and designed according to the parameters. In order to achieve the best polarization effect, the preferred structural parameters of this comb-shaped electrode are: electrode length 25um, tip 5um, period length 3-4um, electrode width 0.8-1um, and positive and negative electrode spacing 6um. The spacing between the positive and negative electrodes has a very large relationship with the size of the applied voltage. At present, under the conditions of this electrode structure, the polarization voltage is preferably in the range of 100-400V, and 370V is further preferred as the optimal polarization voltage.

[0045] The process of etching first and then polarizing provided by the present invention has the following process steps: Figure 2 As shown, it is implemented by the following steps:

[0046] 1) preparing an overlay mark, and using a photolithography method to prepare a waveguide shape profile on the surface of an x-cut lithium niobate film according to the overlay mark;

[0047] 2) etching a waveguide structure on the surface of the x-cut lithium niobate film, removing the electron beam glue, and obtaining a lithium niobate film waveguide;

[0048] 3) According to the overlay marks, a comb-shaped electrode shape profile is prepared on the surface of the x-cut lithium niobate film by photolithography, and a metal electrode is plated on the photolithographic comb-shaped electrode shape profile to obtain an intermediate sample; wherein the comb fingers of the comb-shaped electrode are arranged periodically, the comb fingers are perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers;

[0049] 4) removing the photoresist to obtain a polarized electrode structure;

[0050] 5) Connect the electrode on one side of the comb finger to the positive electrode of the circuit, and the electrode on the other side is grounded, and an electric field is applied to cause the lithium niobate in the area covered by the metal electrode to undergo domain reversal;

[0051] 6) Using dilute hydrochloric acid to remove the electrodes, obtaining a domain flipping structure in the waveguide region;

[0052] 7) Polishing the end face of the waveguide to obtain a lithium niobate thin film superlattice waveguide.

[0053] The specific steps of preparing the overlay mark in step 1) include:

[0054] Using photolithography to prepare an overlay mark photoresist pattern on a sample wafer;

[0055] Plating a layer of metal on the photolithographic sample, wherein the thickness of the metal is 30 to 300 nm;

[0056] The specific steps of preparing the comb-shaped electrode in step 3) include:

[0057] Use acetone or nmp solution to remove the photoresist to obtain the overlay mark.

[0058] According to the overlay marks, the comb finger part outline of the comb-shaped electrode shape outline is prepared on the surface of the x-cut lithium niobate film by using a photolithography method, wherein the comb fingers are perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers;

[0059] A layer of metal electrode is plated on the contour of the photoetched comb finger portion;

[0060] The photoresist is removed to obtain periodically arranged comb-finger electrodes;

[0061] According to the overlay marks, a flat plate portion outline of a comb-shaped electrode is prepared on the surface of the x-cut lithium niobate film by using a photolithography method, wherein the flat plate portion outline covers a portion of the comb-shaped finger electrode;

[0062] A layer of metal electrode is plated on the contour of the photolithographic flat plate to obtain an intermediate sample.

[0063] The process of the above preparation method is described in detail below in conjunction with specific examples.

[0064] Example 1

[0065] a) Prepare an overlay mark photoresist pattern on a sample wafer using ultraviolet lithography.

[0066] b) A layer of 30nm / 70nm thick chromium / gold that is difficult to remove is continuously plated on the photolithographic structure.

[0067] c) Using acetone, remove the photoresist, leaving the metal mark for overlay, and obtain the overlay mark.

[0068] d) Using the overlay marks prepared in step c), an electron beam lithography method is used to prepare an electron beam gel waveguide structure on the surface of the x-cut lithium niobate film.

[0069] e) etching on the structure photolithographically processed in step d) by using ion beam etching.

[0070] f) Using RCA solution, remove the electron beam glue, leaving only the waveguide structure.

[0071] g) The comb-shaped fingers of the polarization electrode are prepared by electron beam lithography on the surface. The period is 4.35um, which has been pre-simulated for the 1550nm waveguide. The comb-shaped electrode length is 25um, the front tip is 5um, the electrode width is 1um, and the distance between the electrodes on both sides is 6um.

[0072] h) A 100nm thick layer of metal electrode nickel is deposited on the photolithographic electrode structure by electron beam evaporation.

[0073] i) Use NMP solution to remove the photoresist, leaving the electrode structure.

[0074] j) The pad part of the polarization electrode is overlaid on the surface using ultraviolet lithography technology, a 150nm nickel structure is electron beam evaporated and the photoresist is removed using NMP solution, thus obtaining a complete structure of the polarization electrode.

[0075] k) Connect the positive electrode to the upper electrode and the ground to the lower electrode, then apply an electric field of about 370V to flip the domains between the electrodes. The result is as follows Figure 3 shown.

[0076] l) Use dilute hydrochloric acid to remove the electrodes to obtain a frequency doubling waveguide structure,

[0077] m) The x-cut lithium niobate film is end-polished to obtain a frequency doubling waveguide structure.

[0078] The prepared waveguide structure is optically tested, such as Figure 5 and Figure 6 As shown, the calculated waveguide loss is 0.27db / cm, 1489.9nm is the frequency doubling point, the fundamental wave power is 0.302mw, the frequency doubling power is 8.82uw, and the normalized efficiency is 1977.55%.

[0079] Example 2

[0080] a) Prepare an overlay mark photoresist pattern on a sample wafer using ultraviolet lithography.

[0081] b) A layer of 30nm / 70nm thick chromium / gold that is difficult to remove is continuously plated on the photolithographic structure.

[0082] c) Using acetone, remove the photoresist, leaving the metal mark for overlay, and obtain the overlay mark.

[0083] d) Using the overlay marks prepared in step c), an electron beam lithography method is used to prepare an electron beam gel waveguide structure on the surface of the x-cut lithium niobate film.

[0084] e) etching on the structure photolithographically processed in step d) by using ion beam etching.

[0085] f) Using RCA solution, remove the electron beam glue, leaving only the waveguide structure.

[0086] g) The comb-shaped fingers of the polarization electrode are prepared by surface overlaying using electron beam lithography. The period is a period that has been pre-simulated for the 1550nm waveguide triple frequency. The minimum spacing is 3.53um, the comb-shaped electrode length is 25um, the front tip is 5um, the electrode width is 1um, and the spacing between the electrodes on both sides is 6um.

[0087] h) A 100nm thick layer of metal electrode nickel is deposited on the photolithographic electrode structure by electron beam evaporation.

[0088] i) Use NMP solution to remove the photoresist, leaving the electrode structure.

[0089] j) The pad part of the polarization electrode is overlaid on the surface using ultraviolet lithography technology, a 150nm nickel structure is electron beam evaporated and the photoresist is removed using NMP solution, thus obtaining a complete structure of the polarization electrode.

[0090] k) Connect the positive electrode to the upper electrode and the ground to the lower electrode, then apply an electric field of about 370V to flip the domains between the electrodes. The result is as follows Figure 4 shown.

[0091] l) Use dilute hydrochloric acid to remove the electrodes and obtain a triple frequency waveguide structure.

[0092] m) The x-cut lithium niobate film is end-polished to obtain a frequency tripling waveguide structure.

[0093] Comparative Example 1

[0094] a) Prepare an overlay mark photoresist pattern on a sample wafer using ultraviolet lithography.

[0095] b) A 30nm / 50nm thick layer of chromium / gold that is difficult to remove is continuously plated on the photolithographic structure.

[0096] c) Using acetone, remove the photoresist, leaving the metal mark for overlay, and obtain the overlay mark.

[0097] d) The comb-shaped fingers of the polarization electrode are prepared by electron beam lithography on the surface. The period is the applicable period of the 1064nm waveguide frequency doubling that has been pre-simulated. The minimum spacing is 3.3um, the comb-shaped electrode length is 25um, the electrode width is 1um, and the spacing between the electrodes on both sides is 6um.

[0098] e) A 100 nm thick layer of metal electrode nickel is deposited on the photolithographic electrode structure by electron beam evaporation.

[0099] f) Use NMP solution to remove the photoresist, leaving the electrode structure.

[0100] g) The pad part of the polarization electrode is overlaid on the surface using ultraviolet lithography technology, a 150nm nickel structure is electron beam evaporated and the photoresist is removed using NMP solution, thus obtaining a complete structure of the polarization electrode.

[0101] h) Connect the positive electrode to the upper electrode and the ground to the lower electrode, then apply an electric field of about 350V to flip the domains between the electrodes.

[0102] i) removing the electrodes using dilute hydrochloric acid to obtain a thin film superlattice structure,

[0103] j) Using the overlay marks prepared in step c), an electron beam lithography method is used to prepare an electron beam gel waveguide structure on the surface of the x-cut lithium niobate film.

[0104] k) etching on the structure photolithographically processed in step d) by using ion beam etching.

[0105] l) Use RCA solution to remove the electron beam glue, leaving only the waveguide structure. The result is as follows Figure 4 shown.

[0106] m) The x-cut lithium niobate film is end-polished to obtain a 1064nm frequency doubling waveguide structure.

[0107] The waveguide prepared in Comparative Example 1 was subjected to electron microscope scanning and confocal imaging, and the characterization image of the side wall of the lithium niobate waveguide under electron microscope was obtained as shown in the figure: Figure 7 As shown, the confocal image of the polarized region is Figure 8 As shown, it can be seen that the side wall of the lithium niobate waveguide prepared by first polarization and then etching is wrinkled, which is mainly due to the loss caused by etching after planning; the domain structure of the polarization area is unevenly arranged, compared with the domain structure of the lithium niobate superlattice waveguide prepared in Examples 1 to 2, Figure 8 The polarization region shown in is of poor quality.

[0108] The embodiment of the present invention uses a single-layer end-face coupled waveguide. In some other implementations, other waveguide forms based on the solution provided by the present invention are also applicable to the present application.

[0109] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a lithium niobate thin film superlattice waveguide, characterized in that: The steps include: 1) preparing an overlay mark, and using a photolithography method to prepare a waveguide shape profile on the surface of an x-cut lithium niobate film according to the overlay mark; 2) etching a waveguide structure on the surface of the x-cut lithium niobate film, removing the electron beam glue, and obtaining a lithium niobate film waveguide; 3) According to the overlay marks, a comb-shaped electrode shape profile is prepared on the surface of the x-cut lithium niobate film by photolithography, and a layer of metal electrode is plated on the photolithographic comb-shaped electrode shape profile to obtain an intermediate sample; wherein the comb fingers of the comb-shaped electrode are arranged periodically, the comb fingers are perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers, and the electrode width is 1 / 4 to 1 / 3 of the period length; 4) removing the photoresist to obtain a polarized electrode structure; 5) Connect the electrode on one side of the comb finger to the positive electrode of the circuit, and the electrode on the other side is grounded, and an electric field is applied to cause the lithium niobate in the area covered by the metal electrode to undergo domain reversal; 6) Using dilute hydrochloric acid to remove the electrodes, obtaining a domain flipping structure in the waveguide region; 7) Polishing the end face of the waveguide to obtain a lithium niobate thin film superlattice waveguide.

2. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 1, characterized in that: The preparation of the overlay mark comprises: Using photolithography to prepare an overlay mark photoresist pattern on a sample wafer; Plating a layer of metal on the photolithographic sample, wherein the thickness of the metal is 30 to 300 nm; Use acetone or nmp solution to remove the photoresist to obtain the overlay mark.

3. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 2, characterized in that: The comb-shaped electrode is 25 um long, the tip of the finger is 5 um long, and the period length is 3-4 um.

4. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 1, characterized in that: The metal electrode is one of aluminum, nickel, chromium or titanium.

5. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 1, characterized in that: The voltage of the applied electric field is 100-400V.

6. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 1 or 2, characterized in that: The method comprises preparing a comb-shaped electrode profile on the surface of the x-cut lithium niobate film by photolithography according to the overlay mark, and plating a layer of metal electrode on the photolithographic comb-shaped electrode profile to obtain an intermediate sample including: According to the overlay marks, the comb finger part outline of the comb-shaped electrode shape outline is prepared on the surface of the x-cut lithium niobate film by using a photolithography method, wherein the comb fingers are perpendicular to the z-axis of the lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of the electrode on one side are pointed fingers, and the comb fingers of the electrode on the other side are flat fingers; A layer of metal electrode is plated on the contour of the photoetched comb finger portion; The photoresist is removed to obtain periodically arranged comb-finger electrodes; According to the overlay marks, a flat plate portion outline of a comb-shaped electrode is prepared on the surface of the x-cut lithium niobate film by using a photolithography method, wherein the flat plate portion outline covers a portion of the comb-shaped finger electrode; A layer of metal electrode is plated on the contour of the photolithographic flat plate to obtain an intermediate sample.

7. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 6, characterized in that: The method for removing the electron beam glue is to use RCA solution for corrosion removal, and the formula of the RCA solution is ammonia water: hydrogen peroxide: water = 1:2:

7.

8. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 6, characterized in that: The photolithography method is electron beam lithography, ultraviolet lithography or a combination of electron beam lithography and ultraviolet lithography; the method for removing the photoresist is to use acetone or N-methylpyrrolidone solution to corrode and remove the photoresist.

9. The method for preparing a lithium niobate thin film superlattice waveguide according to claim 1, characterized in that: The comb fingers of the comb-shaped electrode are arranged periodically, the comb fingers are perpendicular to the z-axis of lithium niobate, the comb fingers of the electrodes on both sides are opposite, and the comb fingers of one electrode are pointed fingers, and the comb fingers of the other electrode are flat fingers. The electrode width is 0.8-1um, and the distance between the positive and negative electrodes is 6um.