Application of a supported catalyst in catalyzing the reductive amination of furfural to prepare furfuralamine
By using titanium dioxide nanosheets as a catalyst supporting metal nanoparticles in the reductive amination reaction of furfural, the problem of low yield of furfurylamine in the existing technology is solved, and efficient preparation of furfurylamine is achieved, with the yield reaching 90.2-95.9% and maintaining Catalyst stability.
Patent Information
- Application Number
- CN202310225239.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-10
AI Technical Summary
In the process of preparing furfurylamine through reductive amination of furfural using existing catalysts, the yield of furfurylamine is low, usually less than 90%.
Titanium dioxide nanosheets are used as carriers to load metal nanoparticles such as Pt, Ru, Pd or Ni, and a supported catalyst is prepared through a reduction reaction, which is used to catalyze the reductive amination reaction of furfural and increase the yield of furfurylamine.
Through this method, the yield of furfurylamine reaches 90.2-95.9%, which significantly improves the yield of furfurylamine, and the catalyst has good stability and can be used repeatedly.
Smart Images

Figure CN116272966B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and particularly relates to application of a supported catalyst in catalyzing the reductive amination of furfural to prepare furfurylamine. Background Art
[0002] Furfural is a degradation product of hemicellulose. Furfural is mainly produced by processing agricultural and forestry wastes such as corn cobs, straw, rice straw and sawdust. Furfural contains a furan ring and an aldehyde group. Its rich functional groups can be converted into high-value chemicals such as furfuryl alcohol, tetrahydrofurfuryl alcohol, 2-methylfuran, furoic acid and furan through hydrogenation, oxidation and decarbonylation. The preparation of furfurylamine by reductive amination of furfural is a new process developed in the field of biomass conversion in recent years, and has gradually attracted the attention of scientific researchers. Furfurylamine has a wide range of uses and is a raw material for many fine chemical products and drugs, such as diuretics; at the same time, furfurylamine can also be used as an anti-corrosion agent.
[0003] Catalysts are required in the process of furfural reductive amination to prepare furfural amine, and the existing catalysts are mainly supported metal catalysts. For example, Japanese scientists Hara et al. (Deng Dian et al., ACS Sustainable Chemistry & Engineering, 2019, 7, 4692-4698) used Ru / Nb2O5·nH2O catalyst to introduce 15mmol furfural into an intermittent reactor, and passed 0.1MPaNH3 and 3MPa H2 into the methanol solution to prepare furfural amine with a yield of 87%. Another example is the Ding Mingyue team of Wuhan University (Dong Chenglong et al., Molecular Catalysis, 2020, 482, 110755) using Ru / HZSM-5 catalyst, methanol as solvent, and preparing furfural amine at a reaction temperature of 100°C, with a yield of 76%. For example, Xu Bingjun et al. (Gould et al., ChemCatChem, 2020, 12, 2106-2115) used SiO2 to load metal catalysts (Pt, Pd, Rh, Ru, Ni and Co), and used dioxane and water as a mixed solvent (mass ratio of 40:1) to prepare furfural amine at a reaction temperature of 130°C, with a yield of 72%. Although the existing catalysts can catalyze the reductive amination reaction of furfural, the yield of furfural amine prepared using the existing catalysts is low, generally less than 90%. Summary of the invention
[0004] In view of this, the present invention provides an application of a supported catalyst in catalyzing the reductive amination of furfural to prepare furfuralamine. The use of the catalyst provided by the present invention as a catalyst for catalyzing the reductive amination of furfural to prepare furfuralamine can greatly improve the yield of furfuralamine.
[0005] In order to solve the above technical problems, the present invention provides an application of a supported catalyst in catalyzing the reductive amination of furfural to prepare furfurylamine, wherein the supported catalyst comprises a carrier and metal nanoparticles supported on the surface of the carrier;
[0006] The carrier is titanium dioxide nanosheets, and the metal nanoparticles include one or more of Pt nanoparticles, Ru nanoparticles, Pd nanoparticles and Ni nanoparticles.
[0007] Preferably, the average particle size of the metal nanoparticles is 1 to 4 nm.
[0008] Preferably, the mass percentage of the metal nanoparticles to the supported catalyst is 0.6-3%.
[0009] Preferably, the specific surface area of the titanium dioxide nanosheets is 50 to 100 m 2 / g.
[0010] Preferably, the method for preparing the supported catalyst comprises the following steps:
[0011] Mixing titanium dioxide nanosheets and a metal nanoparticle precursor solution to obtain a mixed solution; the metal nanoparticle precursor is a metal soluble salt;
[0012] A reducing agent solution is added dropwise to the mixed solution to carry out a reduction reaction, thereby obtaining the supported catalyst.
[0013] Preferably, the molar concentration of the metal nanoparticle precursor solution is 0.001-0.01 mol / L.
[0014] Preferably, the molar concentration of the reducing agent solution is 0.1-0.5 mol / L, and the molar ratio of the reducing agent in the reducing agent solution to the metal in the metal nanoparticle precursor solution is 5-30:1.
[0015] Preferably, the reduction reaction time is 0.5 to 3 hours.
[0016] Preferably, the method for preparing furfurfurylamine by catalytic reductive amination of furfural comprises the following steps:
[0017] Mixing furfural, aqueous ammonia, ethanol and a supported catalyst to obtain a solution to be reacted;
[0018] Hydrogen is introduced into the reaction solution to carry out a reductive amination reaction to obtain the furfurylamine.
[0019] Preferably, the temperature of the reductive amination reaction is 60-120° C., and the time of the reductive amination reaction is 0.5-5 h.
[0020] The present invention provides an application of a supported catalyst in catalyzing the reduction amination of furfural to prepare furfural amine. The supported catalyst comprises a carrier and metal nanoparticles supported on the surface of the carrier; the carrier is a titanium dioxide nanosheet, and the metal nanoparticles comprise one or more of Pt nanoparticles, Ru nanoparticles, Pd nanoparticles and Ni nanoparticles. TiO2 nanosheets are a two-dimensional layered structure material with a large specific surface area. TiO2 nanosheets contain a large number of surface coordination unsaturated sites and oxygen defects, which can be used to anchor metal nanoparticles. Therefore, TiO2 nanosheets can form a strong interaction with metal nanoparticles to form a metal-TiO2 interface, and these interfacial active sites can significantly improve the adsorption and activation ability of the metal / TiO2 catalyst to furfural and NH3. Therefore, the yield of furfural amine is 90.2-95.9% when furfural is catalyzed and reduced by the supported catalyst provided by the present invention to prepare furfural amine, which greatly improves the yield of furfural amine. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a transmission electron microscope (TEM) image of the titanium dioxide nanosheet in Example 1;
[0022] Figure 2 This is the TEM image of the Ru / TiO2 catalyst prepared in Example 1. DETAILED DESCRIPTION
[0023] The invention provides an application of a supported catalyst in catalyzing the reductive amination of furfural to prepare furfurylamine. The supported catalyst comprises a carrier and metal nanoparticles supported on the surface of the carrier.
[0024] In the present invention, the carrier is a titanium dioxide nanosheet; the specific surface area of the titanium dioxide nanosheet is preferably 50 to 100 m 2 / g, more preferably 60 to 80 m 2 / g; the length of the titanium dioxide nanosheet is preferably 80 to 140 nm; the thickness of the titanium dioxide nanosheet is preferably 5 to 7 nm.
[0025] In the present invention, the method for preparing the titanium dioxide nanosheets preferably comprises the following steps:
[0026] The titanium dioxide precursor and hydrofluoric acid are mixed to undergo a hydrothermal reaction to obtain titanium dioxide nanosheets.
[0027] In the present invention, the titanium dioxide precursor is preferably tetraethyl titanate, tetrapropyl titanate or tetrabutyl titanate, and is more preferably tetraethyl titanate. In the present invention, the mass concentration of the hydrofluoric acid is preferably 30 to 50%, and is more preferably 35 to 45%. In the present invention, the volume ratio of the titanium dioxide precursor to the hydrofluoric acid is preferably 3 to 10:1, and is more preferably 4 to 6:1.
[0028] In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring speed is preferably 300-600 r / min, more preferably 400-500 r / min; the stirring time is preferably 8-12 min, more preferably 10 min.
[0029] In the present invention, the temperature of the hydrothermal reaction is preferably 150-300°C, more preferably 200-250°C; the time of the hydrothermal reaction is preferably 12-48h, more preferably 15-40h. In the present invention, the hydrothermal reaction is preferably carried out in a crystallization kettle.
[0030] In the present invention, after the hydrothermal reaction, the method preferably further includes: cooling the system after the hydrothermal reaction and filtering it, and drying the solid obtained by filtration to obtain the titanium dioxide nanosheets. The present invention has no special requirements for the cooling, as long as the system can be cooled to room temperature. In the present invention, the room temperature is preferably 20 to 35°C, more preferably 25 to 30°C. The present invention has no special limitations on the filtration, and conventional methods in the art can be used. The present invention has no special requirements for the drying, as long as the solvent on the surface of the titanium dioxide nanosheets can be removed.
[0031] In the present invention, the metal nanoparticles include one or more of Pt nanoparticles, Ru nanoparticles, Pd nanoparticles and Ni nanoparticles, preferably Pt nanoparticles, Ru nanoparticles, Pd nanoparticles or Ni nanoparticles. In the present invention, the average particle size of the metal nanoparticles is preferably 1 to 4 nm, more preferably 1 to 2 nm. In the present invention, the mass percentage of the metal nanoparticles in the supported catalyst is preferably 0.6 to 3%, more preferably 1 to 2%.
[0032] In the present invention, the method for preparing the supported catalyst preferably comprises the following steps:
[0033] Mixing titanium dioxide nanosheets and a metal nanoparticle precursor solution to obtain a mixed solution; the metal nanoparticle precursor is a metal soluble salt;
[0034] A reducing agent solution is added dropwise to the mixed solution to carry out a reduction reaction, thereby obtaining the supported catalyst.
[0035] The present invention mixes titanium dioxide nanosheets and a metal nanoparticle precursor solution to obtain a mixed solution. In the present invention, the metal nanoparticle precursor solution is preferably a metal salt solution, specifically a RuCl3 solution, a PdCl2 solution, a H2PtCl6 solution or a NiCl2 solution. In the present invention, the molar concentration of the metal nanoparticle precursor solution is preferably 0.001 to 0.01 mol / L, more preferably 0.004 to 0.008 mol / L.
[0036] In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring speed is preferably 300-600 r / min, more preferably 400-500 r / min; the stirring time is preferably 0.5-3 h, more preferably 1-2.5 h; the stirring temperature is preferably room temperature, and the room temperature is preferably 20-35°C, more preferably 25-30°C.
[0037] After obtaining the mixed solution, the present invention drips a reducing agent solution into the mixed solution to carry out a reduction reaction to obtain the supported catalyst. In the present invention, the reducing agent solution is preferably a sodium borohydride solution. In the present invention, the molar concentration of the reducing agent solution is preferably 0.1 to 0.5 mol / L, more preferably 0.2 to 0.4 mol / L. In the present invention, the ratio of the amount of the reducing agent in the reducing agent solution to the amount of the metal in the metal nanoparticle precursor solution is preferably 5 to 30:1, more preferably 10 to 20:1.
[0038] In the present invention, the reduction reaction time is preferably 0.5 to 3 hours, more preferably 1 to 2.5 hours. In the present invention, the reduction reaction is preferably accompanied by stirring, and the stirring speed is preferably 300 to 600 r / min, more preferably 400 to 500 r / min.
[0039] In the present invention, after the reduction reaction, the method preferably further comprises: filtering the system after the reduction reaction, and drying the solid obtained by filtration to obtain the supported catalyst. The present invention has no special requirements for the filtration, and a conventional method in the art can be used. In the present invention, the drying is preferably vacuum drying. The present invention has no special requirements for the vacuum drying, and a conventional method in the art can be used.
[0040] In the present invention, the method for preparing furfurfurylamine by catalytic reductive amination of furfural preferably comprises the following steps:
[0041] Mixing furfural, aqueous ammonia, ethanol and a supported catalyst to obtain a solution to be reacted;
[0042] Hydrogen is introduced into the reaction solution to carry out a reductive amination reaction to obtain the furfurylamine.
[0043] The present invention mixes furfural, ammonia water, ethanol and a supported catalyst to obtain a solution to be reacted. In the present invention, the mass concentration of the ammonia water is preferably 25-30%, more preferably 26-28%. In the present invention, the molar ratio of NH3 in the furfural and ammonia water is preferably 5-30:1, more preferably 10-20:1. In the present invention, the mass ratio of the furfural and the supported catalyst is preferably 100:1-10, more preferably 100:2-6.
[0044] In the present invention, the reductive amination reaction is preferably carried out in a high-pressure reactor. In the present invention, the ethanol is a solvent; the present invention has no special requirements for the amount of the ethanol as long as the solvent can be completely dissolved, and the volume of the ethanol in the present invention is preferably 1 / 3 to 1 / 2 of the volume of the high-pressure reactor. The present invention has no special restrictions on the mixing as long as it can be mixed evenly.
[0045] After obtaining the solution to be reacted, the present invention introduces hydrogen into the solution to be reacted to carry out a reduction amination reaction to obtain the furfurylamine. In the present invention, the pressure of the hydrogen is preferably 2 to 7 MPa, more preferably 3 to 5 MPa. In the present invention, the temperature of the reduction amination reaction is preferably 60 to 120° C., more preferably 80 to 100° C.; the time of the reduction amination reaction is preferably 0.5 to 5 h, more preferably 1 to 3 h.
[0046] In the present invention, the reductive amination reaction is preferably carried out in a high-pressure reactor.
[0047] In the present invention, TiO2 nanosheet is a two-dimensional layered structure material with a large specific surface area. TiO2 nanosheet contains a large number of surface coordination unsaturated sites and oxygen defects, which can be used to anchor metal nanoparticles. Therefore, TiO2 nanosheet can form a strong interaction with metal nanoparticles to form a metal-TiO2 interface. These interfacial active sites can significantly improve the catalytic performance of metal / TiO2 catalyst in furfural reduction amination to prepare furfural amine, improve furfural conversion rate and furfural amine yield. Strong metal-carrier interface in supported catalyst can improve the stability of catalyst and inhibit sintering and deactivation of metal nanoparticles in the reaction process.
[0048] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0049] Example 1
[0050] 5 mL of tetrabutyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 200°C for 24 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0051] 0.2 g of TiO2 nanosheets and 10 mL of RuCl3 solution with a molar concentration of 0.004 mol / L were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 2.37 mL of NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, with stirring at 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a Ru / TiO2 catalyst;
[0052] 5 mmol furfural, 0.9 g ammonia water, 4 mL ethanol and 0.02 g Ru / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa H2 was introduced. The reductive amination reaction was carried out at 90°C for 1.5 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0053] The TiO2 nanosheets were examined by transmission electron microscopy to obtain the TEM image of the TiO2 nanosheets, as shown in Figure 1 As shown. Figure 1 It can be seen that the TiO2 nanosheets present a clear rectangular nanosheet morphology, the length of the TiO2 nanosheets is 80-140nm, and the thickness of the TiO2 nanosheets is 5-7nm. The most exposed crystal plane is the anatase TiO2 (101) crystal plane, and its lattice spacing is 0.35nm. The specific surface area of the TiO2 nanosheets detected by the BET method is 69.3m 2 / g
[0054] The Ru / TiO2 catalyst was tested by transmission electron microscopy to obtain the TEM image of the Ru / TiO2 catalyst, as shown in Figure 2 As shown. Figure 2 It can be seen that Ru nanoparticles are uniformly dispersed on the TiO2 surface, and the average particle size of Ru nanoparticles is 1.6 nm.
[0055] The prepared furfurylamine was analyzed by gas chromatography, and the furfural conversion rate was 95.3%, and the furfurylamine yield was 93.7%.
[0056] The Ru / TiO2 catalyst prepared in Example 1 was used to repeatedly perform catalytic reduction amination reaction. After 5 cycles, the furfural conversion rate was 95.9% and the furfural amine yield was 94.4% as measured by the above method. The Ru / TiO2 catalyst has good stability and can be used repeatedly.
[0057] Example 2
[0058] According to the method of Example 1, a Ru / TiO2 catalyst was prepared;
[0059] The reductive amination reaction was carried out according to the method of Example 1, except that the amount of Ru / TiO2 catalyst used was 0.04 g, the temperature of the reductive amination reaction was 80° C., and the time of the reductive amination reaction was 1 h.
[0060] Example 3
[0061] 5 mL of tetrabutyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 210°C for 20 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0062] 0.2 g of TiO2 nanosheets and 10 mL of a PdCl2 solution with a molar concentration of 0.004 mol / L were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 2.37 mL of a NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, with stirring at 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a Pd / TiO2 catalyst;
[0063] 5 mmol furfural, 0.9 g ammonia water, 4 mL ethanol and 0.03 g Pd / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa H2 was introduced. The reductive amination reaction was carried out at 90°C for 2 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0064] Example 4
[0065] Prepare Pd / TiO2 catalyst according to the method of Example 3;
[0066] 5 mmol of furfural, 1.2 g of ammonia water, 4 mL of ethanol and 0.03 g of Pd / TiO2 catalyst were added to a high-pressure reactor, and 5 MPa of H2 was introduced. The reductive amination reaction was carried out at 95°C for 2 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0067] Example 5
[0068] 5 mL of tetrapropyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 200°C for 30 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0069] 0.4 g of TiO2 nanosheets and 20 mL of H2PtCl6 solution with a molar concentration of 0.004 mol / L were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 4.74 mL of NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, with stirring at 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a Pt / TiO2 catalyst;
[0070] 5 mmol of furfural, 0.8 g of ammonia water, 4 mL of ethanol and 0.02 g of Pt / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa of H2 was introduced. The reductive amination reaction was carried out at 90°C for 1.5 h. After cooling to 25°C, the mixture was centrifuged to obtain furfuralamine.
[0071] Example 6
[0072] Prepare Pt / TiO2 catalyst according to the method of Example 5;
[0073] 5 mmol of furfural, 0.8 g of ammonia water, 4 mL of ethanol and 0.03 g of Pt / TiO2 catalyst were added to a high-pressure reactor, and 5 MPa of H2 was introduced. The reductive amination reaction was carried out at 95°C for 2 h. After cooling to 25°C, the mixture was centrifuged to obtain furfuralamine.
[0074] Example 7
[0075] 5 mL of tetrapropyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 200°C for 30 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0076] 0.4 g of TiO2 nanosheets and 20 mL of NiCl2 solution with a molar concentration of 0.004 mol / L were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 4.74 mL of NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, with stirring at 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a Ni / TiO2 catalyst;
[0077] 5 mmol furfural, 1.1 g ammonia water, 4 mL ethanol and 0.04 g Ni / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa H2 was introduced. The reductive amination reaction was carried out at 90°C for 2 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0078] Example 8
[0079] Prepare Ni / TiO2 catalyst according to the method of Example 7;
[0080] 8 mmol furfural, 1.8 g ammonia water, 6 mL ethanol and 0.08 g Ni / TiO2 catalyst were added to a high-pressure reactor, and 5 MPa H2 was introduced. The reductive amination reaction was carried out at 95°C for 4 h. After cooling to 25°C, the mixture was centrifuged to obtain furfuralamine.
[0081] Example 9
[0082] 5 mL of tetrabutyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 200°C for 30 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0083] 0.4 g of TiO2 nanosheets and 20 mL of a mixed solution of RuCl3 and PdCl2 with a molar concentration of 0.002 mol / L and a molar concentration of 0.002 mol / L were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 4.74 mL of a NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, with stirring at a speed of 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a RuPd / TiO2 catalyst;
[0084] 5 mmol of furfural, 1 g of ammonia water, 4 mL of ethanol and 0.02 g of RuPd / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa of H2 was introduced. The reductive amination reaction was carried out at 90°C for 1.5 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0085] Example 10
[0086] The RuPd / TiO2 catalyst was prepared according to the method of Example 9;
[0087] 10 mmol furfural, 2.5 g ammonia water, 8 mL ethanol and 0.05 g RuPd / TiO2 catalyst were added to a high-pressure reactor, and 6 MPa H2 was introduced. The reductive amination reaction was carried out at 90°C for 3 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0088] Embodiment 11
[0089] 5 mL of tetrabutyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 200°C for 30 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0090] 0.4 g of TiO2 nanosheets and 20 mL of a mixed solution of RuCl3 and H2PtCl6 with a molar concentration of 0.002 mol / L and a molar concentration of 0.002 mol / L were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 4.74 mL of a NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, with stirring at a speed of 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a RuPt / TiO2 catalyst;
[0091] 5 mmol of furfural, 1.2 g of ammonia water, 4 mL of ethanol and 0.04 g of RuPt / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa of H2 was introduced. The reductive amination reaction was carried out at 60°C for 4 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0092] Example 12
[0093] According to the method of Example 11, a RuPt / TiO2 catalyst was prepared;
[0094] 5 mmol of furfural, 1.1 g of ammonia water, 4 mL of ethanol and 0.02 g of RuPt / TiO2 catalyst were added to a high-pressure reactor, and 5 MPa of H2 was introduced. The reductive amination reaction was carried out at 90°C for 1.5 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0095] Embodiment 13
[0096] 5 mL of tetrabutyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 220°C for 24 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0097] 0.4 g of TiO2 nanosheets and 20 mL of a mixed solution of RuCl3 and NiCl2 with a molar concentration of 0.002 mol / L and a molar concentration of 0.002 mol / L, respectively, were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 4.74 mL of a NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, with stirring at a speed of 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a RuNi / TiO2 catalyst;
[0098] 5 mmol of furfural, 0.9 g of ammonia water, 4 mL of ethanol and 0.02 g of RuNi / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa of H2 was introduced. The reductive amination reaction was carried out at 90°C for 1.5 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0099] Embodiment 14
[0100] According to the method of Example 13, a RuNi / TiO2 catalyst was prepared;
[0101] 5 mmol furfural, 1 g ammonia water, 4 mL ethanol and 0.03 g RuNi / TiO2 catalyst were added to a high-pressure reactor, and 5 MPa H2 was introduced. The reductive amination reaction was carried out at 80°C for 2 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0102] Embodiment 15
[0103] 5 mL of tetrabutyl titanate and 1.0 mL of hydrofluoric acid with a mass concentration of 40% were stirred at 400 r / min at 25°C for 10 min and then transferred to a crystallization kettle for hydrothermal reaction at 200°C for 24 h. After cooling to 25°C, the mixture was filtered and dried to obtain TiO2 nanosheets.
[0104] 0.4 g of TiO2 nanosheets and 20 mL of a mixed solution of H2PtCl6 and NiCl2 with a molar concentration of 0.002 mol / L and a molar concentration of 0.002 mol / L of H2PtCl6 and NiCl2 were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 4.74 mL of a NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, and the addition was accompanied by stirring at a speed of 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a PtNi / TiO2 catalyst;
[0105] 5 mmol furfural, 1.2 g ammonia water, 4 mL ethanol and 0.02 g PtNi / TiO2 catalyst were added to a high-pressure reactor, and 5 MPa H2 was introduced. The reductive amination reaction was carried out at 90°C for 1.5 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0106] Example 16
[0107] Prepare PtNi / TiO2 catalyst according to the method of Example 15;
[0108] 5 mmol of furfural, 1.55 g of ammonia water, 4 mL of ethanol and 0.03 g of PtNi / TiO2 catalyst were added to a high-pressure reactor, and 6 MPa of H2 was introduced. The reductive amination reaction was carried out at 70°C for 2 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0109] Comparative Example 1
[0110] 0.2 g of commercially available TiO2 (purchased from Shentai Chemical Reagent Co., Ltd.) and 10 mL of RuCl3 solution with a molar concentration of 0.004 mol / L were stirred at 400 r / min for 1 h at 25°C to obtain a mixed solution; 2.37 mL of NaBH4 solution with a molar concentration of 0.25 mol / L was added dropwise to the mixed solution within 0.5 h, accompanied by stirring at a speed of 400 r / min; after filtering, the filtered solid was vacuum dried to obtain a Ru / TiO2 catalyst;
[0111] 5 mmol furfural, 0.9 g ammonia water, 4 mL ethanol and 0.02 g Ru / TiO2 catalyst were added to a high-pressure reactor, and 4 MPa H2 was introduced. The reductive amination reaction was carried out at 90°C for 1.5 h. After cooling to 25°C, the mixture was centrifuged to obtain furfural amine.
[0112] The furfural amine prepared in Examples 1 to 16 and Comparative Example 1 was analyzed by gas chromatography, and the results of furfural conversion rate and furfural amine yield are listed in Table 1.
[0113] Table 1 Furfural conversion rate and furfurylamine yield in Examples 1 to 16 and Comparative Example 1
[0114]
[0115]
[0116] It can be seen from the result data of Example 1 and Comparative Example 1 in Table 1 that the supported catalyst prepared using TiO2 nanosheets as a carrier has good catalytic performance for the reductive amination of furfural to prepare furfuralamine, and significantly improves the conversion rate of furfural and the yield of furfuralamine.
[0117] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. Use of a supported catalyst in catalyzing the reductive amination of furfural to prepare furfurylamine, the supported catalyst comprising a carrier and metal nanoparticles supported on the surface of the carrier; The carrier is a titanium dioxide nanosheet, and the specific surface area of the titanium dioxide nanosheet is 50-100 m 2 / g; the metal nanoparticles include one or more of Pt nanoparticles, Ru nanoparticles, Pd nanoparticles and Ni nanoparticles; The preparation method of the titanium dioxide nanosheets comprises the following steps: A titanium dioxide precursor and hydrofluoric acid are mixed to undergo a hydrothermal reaction to obtain titanium dioxide nanosheets; The titanium dioxide precursor is tetraethyl titanate, tetrapropyl titanate or tetrabutyl titanate; the mass concentration of the hydrofluoric acid is 30-50%; the volume ratio of the titanium dioxide precursor to the hydrofluoric acid is 3-10:1; The temperature of the hydrothermal reaction is 150-300° C., and the time of the hydrothermal reaction is 12-48 hours.
2. The application according to claim 1, characterized in that: The average particle size of the metal nanoparticles is 1-4 nm.
3. The use according to claim 1 or 2, characterized in that: The mass percentage of the metal nanoparticles in the supported catalyst is 0.6-3%.
4. The use according to claim 1, characterized in that: The method for preparing the supported catalyst comprises the following steps: Mixing titanium dioxide nanosheets and a metal nanoparticle precursor solution to obtain a mixed solution; the metal nanoparticle precursor is a metal soluble salt; A reducing agent solution is added dropwise to the mixed solution to carry out a reduction reaction, thereby obtaining the supported catalyst.
5. The application according to claim 4, characterized in that: The molar concentration of the metal nanoparticle precursor solution is 0.001-0.01 mol / L.
6. The use according to claim 4 or 5, characterized in that: The molar concentration of the reducing agent solution is 0.1-0.5 mol / L, and the molar ratio of the reducing agent in the reducing agent solution to the metal in the metal nanoparticle precursor solution is 5-30:
1.
7. The use according to claim 4, characterized in that: The reduction reaction time is 0.5 to 3 hours.
8. The use according to claim 1, characterized in that: The method for preparing furfurfurylamine by catalytic reductive amination of furfural comprises the following steps: Mixing furfural, aqueous ammonia, ethanol and a supported catalyst to obtain a solution to be reacted; Hydrogen is introduced into the reaction solution to carry out a reductive amination reaction to obtain the furfurylamine.
9. The use according to claim 8, characterized in that: The temperature of the reductive amination reaction is 60-120° C., and the time of the reductive amination reaction is 0.5-5 h.
Citation Information
Cited By
Catalyst taking thermal cracking carbon black as carrier as well as preparation method and application of catalyst
CN120861087A