Preparation method and application of in-situ self-lubricating aluminum-based armature
The mechanical mixing and hot extrusion process of nanometal sulfide and aluminum alloy is prepared by hydrothermal method to form a multi-composite compound protective layer, solving the friction and wear problem of armature materials under extreme working conditions, and achieving low density and high strength and high conductivity aluminum-based armatures, significantly reducing friction and wear performance.
Patent Information
- Application Number
- CN202310283083.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-22
AI Technical Summary
In the existing electromagnetic propulsion technology, armature materials are prone to friction wear, edge groove corrosion, arc ablation and other damages under extreme service conditions, and existing self-lubricating materials will damage the mechanical properties of the aluminum alloy matrix, making it difficult to take into account the conductivity. and friction wear performance.
The nano-metal sulfide powder is prepared by hydrothermal method and mechanically mix it with aluminum alloy powder, add metal magnesium powder, and perform cold isostatic molding and sintering. The C-type or U-type armature is prepared by hot extrusion process to form nano-sulfide and The multi-composite compound protective layer of magnesium element prevents reaction and partial aggregate and improves interface binding strength.
Low-density, high-strength, self-lubricating aluminum-based armatures are realized, which significantly reduces friction and wear performance, improves conductive and mechanical properties, has high material utilization, high manufacturing efficiency and low cost.
Smart Images

Figure CN116275046B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powder metallurgy aluminum-based composite materials, and in particular to a preparation method and application of an in-situ self-lubricating aluminum-based armature. Background Art
[0002] Electromagnetic propulsion technology is a new type of propulsion technology that uses electromagnetic force to accelerate objects to ultra-high speeds. Compared with conventional chemical propulsion methods, electromagnetic propulsion can provide greater kinetic energy, and can accelerate the armature and moving body to an ultra-high initial velocity that is difficult to achieve with chemical propulsion methods. It also has the advantages of arbitrarily controllable speed and the launch process is not easily interfered with. Therefore, it has extremely broad and far-reaching application prospects in various types of national defense weapons, transportation, and aerospace fields.
[0003] At present, the development of electromagnetic propulsion technology is still in the laboratory stage. One of the main problems is that the armature / rail materials currently used cannot meet extreme service conditions. As a key component of the electromagnetic railgun, the armature plays an important role in carrying current and propelling the projectile. In the process of the electromagnetic railgun firing the armature, the electromagnetic force generated by the pulsed large current on the armature can accelerate the projectile from static to hundreds of meters per second in a very short time, or even to thousands of meters per second. At this time, the sliding electrical contact between the armature and the rail is very bad, and complex mechanical, thermal, electrical effects and strong side impact forces will occur between the armature / rail interface, causing material softening, friction wear, edge groove corrosion, high-speed planing, arc ablation and other damage. It can be seen that the quality of the armature performance directly affects the service life of the rail.
[0004] The existing technology for preparing high-strength and high-conductivity aluminum alloy armature materials improves the conductivity of 7XXX series aluminum alloys by adding micro-alloyed precious metal elements (Zr, Ag, Y) and combining long-term multi-stage aging. However, the production cost is high and the manufacturing cycle is long, resulting in high production costs. Alternatively, in order to avoid the reaction of aluminum alloys with existing solid lubricants, high entropy alloy TiCoCrFeNiAl is added to coat MoS 2 However, since the added particles are in the micron scale, the mechanical properties of the aluminum alloy matrix are seriously damaged.
[0005] In order to improve the friction and wear performance of aluminum alloy armatures, coating the surface of solid lubricants such as molybdenum disulfide and tungsten disulfide without reducing the mechanical properties of the armature has always been a difficult problem that needs to be solved urgently in the armature field. Summary of the invention
[0006] The preparation method and application of the in-situ self-lubricating aluminum-based armature provided by the present invention can not only solve the problem of reaction between the lubricating phase and the matrix, but also improve the interface bonding. On the basis of ensuring excellent conductive properties, it has the characteristics of low density, high strength and self-lubrication.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] A method for preparing an in-situ self-lubricating aluminum-based armature, comprising:
[0009] Step S1, using ammonium metal acid and thiourea as raw materials, preparing nano metal sulfide (i.e., Me x S y )powder;
[0010] Step S2: Nano-Me x S y Powder, metal magnesium powder and aluminum alloy powder are mechanically mixed to obtain nano-Me x S y / aluminum alloy composite powder; at this time, the magnesium powder and the aforementioned aluminum alloy powder are composited to form a new aluminum alloy powder component system;
[0011] Step S3, encapsulating the composite powder and obtaining a green body by cold isostatic pressing;
[0012] Step S4, placing the green body in a sintering furnace for sintering to obtain a sintered ingot of the aluminum-based composite material;
[0013] Step S5: using a hot extrusion process to extrude the aluminum-based composite material sintered ingot into a C-shaped or U-shaped armature to obtain a fully dense, high-strength, high-conductivity, self-lubricating aluminum-based armature.
[0014] Optionally, step S1 specifically includes: adding ammonium metal acid and thiourea to water to completely dissolve them, then mixing the two solutions evenly, adding acid to adjust the pH to below 3, transferring the solution into a reaction vessel lined with polytetrafluoroethylene, heating the reaction at a suitable temperature, then naturally cooling to room temperature, rinsing, drying, and grinding to obtain nano-Me x S y powder.
[0015] Optionally, in step S1, the metal Me is selected from one or more of W, Mo, Mn, Cu, Zn, and Sn, and the values of x and y are determined according to Me, that is, the composition of the metal sulfide is determined according to the selection of the metal.
[0016] Optionally, in step S1, the concentration of ammonium metal acid and the concentration of thiourea are 0.01-2 mol / L and 0.1-5 mol / L respectively, the hydrothermal reaction temperature is 100-300°C, the time is 5-48h, and the drying temperature is 30-200°C.
[0017] Nano-sized sulfide powder can only be obtained by strictly controlling the key process parameters of the hydrothermal synthesis method, such as reactant concentration, pH value, and heating temperature. Improper pH control may make it difficult to generate nano-sulfide powder; too high or too low hydrothermal reaction temperature will cause the sulfide powder particle size to grow significantly.
[0018] Optionally, in step S2, mechanical mixing is ball milling in a ball milling jar with acetone as a process control agent; the ball milling can be planetary ball milling, rolling ball milling or stirring ball milling, the ball milling time is 2-48h, and the ball-to-material ratio should be between 5:1 and 20:1. The ball milling atmosphere is one or both of nitrogen and argon; the amount of mixed metal magnesium added is between 0.1-10wt% of the total amount. The amount of magnesium added ensures that the magnesium element can be x S y In Me x S y A nano-protective layer is formed on the surface to prevent the aggregation and growth and stop it from reacting with the aluminum matrix.
[0019] Optionally, in step S3, cold isostatic pressing is performed at a pressure of 50-400 MPa for 10 seconds to 10 minutes.
[0020] Optionally, in step S4, the sintering method is one or more of spark plasma sintering, vacuum sintering, and atmosphere protection sintering, the sintering temperature is 450-630°C, and the holding time is 5min-5h. During the sintering process, the magnesium element will segregate toward the transition metal sulfide and react with it to form a layer of multi-component composite compound on its surface. Depending on the sintering temperature, sintering time, and element content, the thickness of the reaction layer is 5-20nm.
[0021] During the sintering process, the metallic magnesium element is concentrated on the surface of the nano-sulfide lubricating phase and reacts to form a multi-component composite compound protective layer with a thickness of 5-20nm and controllable thickness, which effectively prevents the Me x S y It reacts with the aluminum alloy matrix and improves the interface bonding. The magnesium content, sintering temperature and holding time need to be precisely controlled, otherwise the sulfide particles may aggregate and grow, and may completely react with the magnesium element to form MgS, which will have a serious adverse effect on the friction and wear performance of the armature.
[0022] Optionally, in step S5, the hot extrusion temperature should be 200-550°C, and hot extrusion is performed after the temperature of the blank is uniform, with an extrusion ratio of 2:1 to 20:1.
[0023] Directly preparing C-shaped or U-shaped armatures through hot extrusion process can not only produce the required shape and specifications, but also further enhance the strength of the armature material and significantly improve the friction and wear performance of the armature.
[0024] Furthermore, the present invention also provides an in-situ self-lubricating aluminum-based armature, a nano-Me x S y The mass fraction of the lubricating phase is 0.1%-5%, the mass fraction of metal magnesium is 0.1%-10%, and the rest is aluminum and other alloy elements; Nano-Me x S y The particle size is 20-100nm and is evenly distributed in the aluminum matrix in the form of a self-lubricating phase.
[0025] Furthermore, the present invention also provides the application of high-strength and high-conductivity self-lubricating aluminum-based armature in electromagnetic propulsion.
[0026] The beneficial effects brought about by the technical solution provided by the present invention include at least:
[0027] The present invention prepares nano-Me by hydrothermal method x S y The lubricating phase powder particles, the prepared nano-sulfide has stable and uniform size and is easy to prepare in batches; it is evenly mixed with aluminum alloy powder and metal magnesium powder by ball milling, and high-performance self-lubricating aluminum-based armature is obtained through cold isostatic pressing, sintering densification and hot extrusion processes. x S y The self-lubricating phase is dispersed in the aluminum alloy matrix and reacts with magnesium during sintering to form a layer of multi-component composite compound on its surface to prevent the sulfide particles from segregating and growing and reacting with the aluminum alloy matrix, improve the interface bonding strength, and make the composite material have low density, high strength and high conductivity, as well as excellent friction and wear properties. x S y The lubricating phase and metallic magnesium are evenly distributed in the aluminum alloy matrix. Through process control, nano-Me x S y The composite material prepared by the controlled reaction with magnesium element has excellent mechanical properties, electrical conductivity and friction and wear properties. By manufacturing the armature in a near-net shape, the material utilization rate is high, the manufacturing efficiency is high, the cost is low, and continuous production can be achieved. The method of the present invention has important application prospects in the field of armatures for electromagnetic propulsion. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 It is a schematic diagram of the process flow of the present invention;
[0030] Figure 2 This is a TEM photograph of nano-molybdenum disulfide particles in the aluminum-based armature microstructure of Example 1 of the present invention. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0032] Example 1
[0033] 1) 4000g (NH 4 ) 2 MoO 4 With 4000g CH 4 N 2 S was put into two beakers, and then 50L of deionized water was added respectively, and magnetic stirring was performed for 30 minutes until it was completely dissolved; then the above two solutions were mixed, and stirring was continued for 20 minutes to make them evenly mixed; concentrated hydrochloric acid was added to adjust the pH of the solution to 2.5, and finally the solution was transferred to a polytetrafluoroethylene reaction liner and kept warm at 230°C for 48 hours; after the reaction was completed, it was cooled to room temperature, washed repeatedly with alcohol and deionized water for three times, excess solution and impurities were filtered out, and the powdered nano molybdenum disulfide was obtained by drying in a drying oven.
[0034] 2) The molybdenum disulfide powder, magnesium metal powder and 7075 aluminum alloy powder were weighed in a mass ratio of 2:5:93, and were ball-milled under argon protection at a ball-to-material ratio of 5:1, a ball milling speed of 300 r / min and a ball milling time of 12 h to finally obtain a composite powder.
[0035] 3) The composite powder was placed in a silica gel bag and vibrated, and the bag was sealed and placed in a cold isostatic press, and the pressure was maintained at 180 MPa for 2 minutes to obtain a sample green body with a diameter of 600 mm and a height of 800 mm. The sample green body was placed in a vacuum sintering furnace and sintered in an argon atmosphere with a gas flow rate of 5 L / min, a sintering temperature of 600°C, and a sintering time of 2 hours to obtain a sintered ingot.
[0036] 4) The aluminum ingot is heated to 370° C. and hot extruded into a steel mold at an extrusion ratio of 16:1 to form a U-shaped armature, thereby obtaining a fully dense, high-strength, high-conductivity aluminum-based self-lubricating armature.
[0037] 5) After heat treatment, the room temperature tensile strength of the armature reaches 637 MPa, and the conductivity is 38% IACS; the average friction coefficient measured by the friction and wear test with the prepared aluminum-based armature using Cu-Cr-Zr copper alloy as the track material is 0.13, and the average friction coefficient measured using the traditional 7075 aluminum alloy is 0.34. The friction coefficient of the armature prepared by the present invention is reduced by 62%.
[0038] Example 2
[0039] 1) 3000g (NH 4 )MnO 4 With 3000g CH 4 N 2 S is put into two beakers, and then 30L of deionized water is added, and magnetic stirring is performed for 30 minutes until it is completely dissolved; then the above two solutions are mixed, and stirring is continued for 20 minutes to make them evenly mixed; concentrated hydrochloric acid is added to adjust the pH of the solution to 2.5, and finally the solution is transferred to a polytetrafluoroethylene reaction liner and kept warm at 250°C for 48 hours; after the reaction is completed, it is cooled to room temperature, and repeatedly washed with alcohol and deionized water for three times, excess solution and impurities are filtered out, and it is placed in a drying oven for drying to obtain powdered nano manganese sulfide.
[0040] 2) The manganese sulfide powder, magnesium metal powder and 7050 aluminum alloy powder were weighed in a mass ratio of 5:5:90, and were ball-milled under argon protection at a ball-to-material ratio of 10:1, a ball milling speed of 500 r / min and a ball milling time of 12 h to finally obtain a composite powder.
[0041] 3) The composite powder was placed in a silica gel bag and vibrated, and the bag was sealed and placed in a cold isostatic press, and the pressure was maintained at 180 MPa for 2 minutes to obtain a sample green body with a diameter of 600 mm and a height of 800 mm. The sample green body was placed in a vacuum sintering furnace and sintered in an argon atmosphere with a gas flow rate of 5 L / min, a sintering temperature of 600°C, and a sintering time of 2 hours to obtain a sintered ingot.
[0042] 4) The aluminum ingot is heated to 370° C. and hot extruded into a steel mold at an extrusion ratio of 16:1 to form a U-shaped armature, thereby obtaining a fully dense, high-strength, high-conductivity aluminum-based self-lubricating armature.
[0043] 5) After heat treatment, the room temperature tensile strength of the armature reaches 682MPa, and the conductivity is 35%LACS; the average friction coefficient measured by the friction and wear test with the prepared aluminum-based armature using Cu-Cr-Zr copper alloy as the track material is 0.12, and the average friction coefficient measured using the traditional 7050 aluminum alloy is 0.3. The friction coefficient of the armature prepared by the present invention is reduced by 60%.
[0044] Example 3
[0045] 1) 5000g (NH 4 ) 6 W 7 O 24 6H 2 O and 3000g CH 4 N 2 S was put into two beakers, and then 50L of deionized water was added, and magnetic stirring was performed for 30 minutes until it was completely dissolved; then the above two solutions were mixed, and stirring was continued for 20 minutes to make them evenly mixed; concentrated hydrochloric acid was added to adjust the pH of the solution to 2, and finally the solution was transferred to a polytetrafluoroethylene reaction liner and kept warm at 270°C for 48 hours; after the reaction was completed, it was cooled to room temperature, washed repeatedly with alcohol and deionized water for three times, the excess solution and impurities were filtered out, and the powdered nano-tungsten sulfide was obtained in a drying oven.
[0046] 2) The manganese sulfide powder, magnesium metal powder and 7055 aluminum alloy powder were weighed in a mass ratio of 5:5:90, and were ball-milled under argon protection at a ball-to-material ratio of 5:1, a ball milling speed of 600 r / min and a ball milling time of 8 h to finally obtain a composite powder.
[0047] 3) The composite powder was placed in a silica gel bag and vibrated, and the bag was sealed and placed in a cold isostatic press, and the pressure was maintained at 180 MPa for 2 minutes to obtain a sample green body with a diameter of 600 mm and a height of 800 mm. The sample green body was placed in a vacuum sintering furnace and sintered in an argon atmosphere with a gas flow rate of 5 L / min, a sintering temperature of 600°C, and a sintering time of 2 hours to obtain a sintered ingot.
[0048] 4) The aluminum ingot is heated to 370° C. and hot extruded into a steel mold at an extrusion ratio of 16:1 to form a C-shaped armature, thereby obtaining a fully dense, high-strength, high-conductivity aluminum-based self-lubricating armature.
[0049] 5) After heat treatment, the room temperature tensile strength of the armature reaches 709 MPa, and the conductivity is 34% IACS; the average friction coefficient measured by the friction and wear test with the prepared aluminum-based armature using Cu-Cr-Zr copper alloy as the track material is 0.12, and the average friction coefficient measured using the traditional 7055 aluminum alloy is 0.39. The friction coefficient of the armature prepared by the present invention is reduced by 69%.
[0050] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing an in-situ self-lubricating aluminum-based armature, characterized in that: include: Step S1, using ammonium metal acid and thiourea as raw materials, preparing nano metal sulfide powder by a hydrothermal method; Step S2, mechanically mixing the nano metal sulfide powder, the metal magnesium powder and the aluminum alloy powder to obtain a nano metal sulfide / aluminum alloy composite powder; Step S3, encapsulating the composite powder and obtaining a green body by cold isostatic pressing; Step S4, placing the green body in a sintering furnace for sintering to obtain a sintered ingot of the aluminum-based composite material; Step S5, using a hot extrusion process to extrude the aluminum-based composite material sintered ingot into a C-shaped or U-shaped armature to obtain a fully dense, high-strength, high-conductivity, self-lubricating aluminum-based armature; In step S1, the metal is selected from one or more of W, Mo, Mn, Cu, and Zn; The mass fraction of the nano-metal sulfide lubricating phase is 0.1%-5%, the mass fraction of metal magnesium is 5%-10%, and the rest is aluminum and other alloying elements; the particle size of the nano-metal sulfide is 20-100 nm, and it is evenly distributed in the aluminum matrix in the form of a self-lubricating phase; Step S1 specifically comprises: adding ammonium metal acid and thiourea into water to completely dissolve them, then mixing the two solutions evenly, adding acid to adjust the pH to below 3, transferring the solution into a reaction vessel lined with polytetrafluoroethylene, heating the reaction at a suitable temperature, then naturally cooling to room temperature, rinsing, drying, and grinding to obtain nano metal sulfide powder; In step S1, the concentration of ammonium metal acid and the concentration of thiourea are 0.01-2 mol / L and 0.1-5 mol / L respectively, the hydrothermal reaction temperature is 100-300°C, the time is 5-48 h, and the drying temperature is 30-200°C; In step S4, the sintering method is one or more of spark plasma sintering, vacuum sintering, and atmosphere protection sintering, the sintering temperature is 450-630°C, and the holding time is 5min-5h; during the sintering process, the magnesium element will segregate toward the transition metal sulfide and react with it to form a layer of multi-component composite compound on its surface with a thickness of 5-20 nm.
2. The method according to claim 1, characterized in that In step S2, mechanical mixing is ball milling in a ball mill using acetone as a process control agent; the ball milling is planetary ball milling, rolling ball milling or stirring ball milling, the ball milling time is 2-48 h, and the ball-to-material ratio should be between 5:1 and 20:1; the ball milling atmosphere is one or both of nitrogen and argon; the amount of mixed metal magnesium added is between 5-10 wt% of the total amount.
3. The method according to claim 1, characterized in that In step S3, cold isostatic pressing is performed at a pressure of 50-400 MPa for 10 s-10 min.
4. The method according to claim 1, characterized in that: In step S5, the hot extrusion temperature should be 200-550°C, and hot extrusion is performed after the temperature of the blank is uniform, and the extrusion ratio is 2:1 to 20:
1.
5. An in-situ self-lubricating aluminum-based armature prepared according to the method according to any one of claims 1 to 4.
6. Application of the in-situ self-lubricating aluminum-based armature as claimed in claim 5 in electromagnetic propulsion.