A method for resource disposal of beryllium-containing silicon slag and its application
By roasting beryllium-containing silicon slag and reducing coal auxiliary materials at a specific temperature, the problems of poor solid beryllium effect and high cost are solved, and safe and efficient curing treatment is achieved. The products can be used in cement clinker to meet green disposal standards.
Patent Information
- Application Number
- CN202310071987.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-07
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-02-07
AI Technical Summary
In the prior art, the solid beryllium-containing silicon slag is poor after treatment, the cost is high, and the process flow is complex, and there is a problem of secondary pollution.
Mix beryllium-containing silicon slag with reducing coal auxiliary materials, roast at 850°C to 1300°C, reduce the transition temperature of beryllium sulfate through a carbon reducing atmosphere, improve the curing efficiency, and ensure the reaction by controlling the calcining temperature and time. Enough to reduce energy consumption.
It achieves low-cost, safe and efficient curing of beryllium-containing silicon slag without secondary pollution. The product has low toxic beryllium content. It is suitable for cement clinker blends and meets the requirements of green disposal.
Smart Images

Figure BDA0004065004080000071
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid waste disposal, and in particular relates to a resource disposal method and application of beryllium-containing silicon slag. Background Art
[0002] Industrial beryllium oxide is mainly produced by the sulfuric acid method. A large amount of beryllium-containing waste slag is generated during the production process. According to the different slag production links, there are mainly four types of environmental slag, silicon slag, iron slag, and aluminum ammonium alum slag. Silicon slag is a glassy body obtained by smelting beryllium ore, which is ground to 200 mesh, mixed with concentrated sulfuric acid, and reacted at 250-300°C to convert beryllium and aluminum oxides into water-soluble sulfates, while silicon dioxide does not react with sulfuric acid to obtain slag. Relevant researchers have conducted certain research on the disposal of beryllium-containing waste slag, but the results are not ideal, and there are shortcomings such as poor beryllium solidification effect and high cost. Therefore, it is of great significance to carry out research on the harmless technology of resource utilization of beryllium-containing silicon slag, solve the storage problem of beryllium-containing waste slag, realize the safe and efficient disposal of beryllium-containing waste slag, and provide technical support for the safe disposal of beryllium-containing waste slag nationwide, while it will escort the sustainable development of the military products industry.
[0003] CN109453493A discloses a stabilizing agent for treating waste residue containing beryllium, and its preparation method and application. The process technology of the invention patent application is to add fly ash, sepiolite and other conditioning agents, calcium oxide, superphosphate and other additives and curing agents to the waste residue containing beryllium to stabilize the waste residue containing beryllium. The process flow is complicated and the reserve of waste residue containing beryllium is increased. CN110252761A discloses a method for harmless treatment of waste residue containing beryllium. The method melts the waste residue containing beryllium and metal tailings at high temperature to vitrify the waste residue containing beryllium. The melting temperature of the process is high and the cost is high. Summary of the invention
[0004] In order to overcome the technical problems of poor beryllium solidification effect and high cost after treatment of beryllium-containing silicon slag in the prior art, the present invention provides a resource disposal method and application of beryllium-containing silicon slag, which has a simple disposal process, low equipment investment, low operating cost, good solidification effect of roasting products, and no secondary pollution, and meets the requirements of safe, efficient and green disposal of beryllium-containing silicon slag.
[0005] In order to solve the above technical problems, the technical solutions proposed by the present invention are as follows:
[0006] A first aspect of the present invention provides a resource disposal method for beryllium-containing silicon slag, wherein the disposal method comprises uniformly mixing the beryllium-containing silicon slag with auxiliary materials and then calcining the mixture at 850° C. to 1300° C. to obtain a calcined sample.
[0007] In the present invention, the calcination temperature of beryllium-containing silicon slag and auxiliary materials is set to 850°C-1300°C. If the calcination temperature is lower than 850°C, the reaction will be insufficient and the beryllium solidification effect will not meet the toxicity leaching requirements; if the calcination temperature is higher than 1300°C, sintering will occur and energy consumption will increase.
[0008] As an optional implementation, in the resource recovery method provided by the present invention, the roasting temperature is 850°C to 1200°C.
[0009] As an optional implementation, in the resource recovery method provided by the present invention, the roasting temperature is 900°C to 1100°C.
[0010] The auxiliary material is a kind of reducing coal, wherein the fixed carbon content is greater than 55% and the calorific value is greater than 4000 kcal / kg.
[0011] In the present invention, auxiliary materials are added to beryllium-containing silicon slag for roasting treatment, wherein the auxiliary materials are a substance that changes the reaction mode, improves the efficiency of solid beryllium, reduces the solid beryllium temperature, and improves the sulfate desulfurization rate. During the roasting treatment process of the auxiliary materials and beryllium-containing silicon slag, the carbon in the auxiliary materials causes the roasting to be carried out in a reducing atmosphere, and the reducing atmosphere is conducive to the decomposition of beryllium sulfate and other sulfates, and reduces the reaction temperature of beryllium sulfate being converted into beryl. First, the carbon in the auxiliary materials can reduce the roasting temperature of beryllium-containing silicon slag, making it easier to undergo phase transformation reconstruction, increase the phase transformation ratio of beryllium sulfate into beryl phase, reduce the leaching toxic beryllium content, and play a role in solid beryllium; secondly, roasting with the addition of auxiliary material carbon can reduce the S content in beryllium-containing silicon slag, allowing S to enter the flue gas in the form of gaseous SO2, which plays a role in reducing the desulfurization roasting temperature and improving the desulfurization efficiency. The reduction of sulfur in the roasted slag can increase the proportion of the roasted sample as cement clinker.
[0012] The amount of the auxiliary material added is 4-12% of the mass of the beryllium-containing silicon slag.
[0013] In the present invention, if the weight ratio of auxiliary materials added to the beryllium-containing silicon slag is less than 4%, the reaction will be incomplete and some of the beryllium-containing silicon slag will remain unreacted; if the weight ratio of auxiliary materials added to the beryllium-containing silicon slag is higher than 12%, some of the auxiliary materials will remain unreacted and too much auxiliary materials will remain; therefore, the weight ratio of auxiliary materials added to the beryllium-containing silicon slag is 4% to 12%.
[0014] As an optional implementation, in the resource recovery disposal method provided by the present invention, the amount of the auxiliary material added is 4-10% of the mass of the beryllium-containing silicon slag.
[0015] As an optional implementation, in the resource recovery disposal method provided by the present invention, the amount of the auxiliary material added is 4-8% of the mass of the beryllium-containing silicon slag.
[0016] As an optional embodiment, in the resource recovery method provided by the present invention, the beryllium-containing silicon slag is obtained by mixing beryllium ore with concentrated sulfuric acid after smelting in the beryllium oxide production process, and reacting at 250-300°C without reacting with sulfuric acid.
[0017] As an optional implementation, in the resource recovery method provided by the present invention, the beryllium-containing silicon slag has a beryllium content of less than 0.2%, a sulfur content of less than 15%, a silicon dioxide content of more than 30%, and a calcium oxide content of more than 10% by weight, which is a hazardous waste.
[0018] In the present invention, beryllium in the beryllium-containing silicon slag is determined by ICP alkali fusion method, S is determined by high-frequency infrared absorption method, SiO2 is determined by perchloric acid dehydration weight method, and CaO is determined by atomic absorption spectrometry.
[0019] As an optional implementation, in the resource recovery disposal method provided by the present invention, the moisture content of the beryllium-containing silicon slag is 30% to 40%.
[0020] As an optional implementation, in the resource recovery method provided by the present invention, the beryllium-containing silicon slag and auxiliary materials are roasted in a muffle furnace, and the power of the muffle furnace is 10 kW to 20 kW.
[0021] The muffle furnace used in the present invention is a box-type muffle furnace, which is a product currently sold on the market, such as a product sold under the trade name of exhaust-type high-temperature muffle furnace. The power of the box-type muffle furnace used in the present invention should be selected according to the heating rate.
[0022] As an optional implementation, in the resource recovery method provided by the present invention, the roasting time is 30 to 60 minutes.
[0023] In the present invention, the calcination time is set to 30 to 60 minutes. If the calcination time is less than 30 minutes, the reaction will be incomplete; if the calcination time is longer than 60 minutes, excessive unnecessary energy consumption will be generated.
[0024] As an optional implementation, in the resource recovery method provided by the present invention, the roasting time is 45 to 60 minutes.
[0025] As an optional implementation, in the resource recovery disposal method provided by the present invention, the content of toxic beryllium leached from the roasted sample is less than 0.00667 mg / L.
[0026] In the roasted sample obtained after roasting in the present invention, the content of leached toxic beryllium is less than 0.02 mg / L, which meets the treatment standard. The basic phase composition of beryllium is beryl, beryllium sulfate and beryllium silicate, and the beryllium in the product mainly exists in the form of beryl.
[0027] A second aspect of the present invention provides an application of the above-mentioned resource disposal method of beryllium-containing silicon slag in the preparation of cement clinker admixtures, specifically, the roasted sample obtained after the treatment is used to prepare cement clinker admixtures.
[0028] As an optional implementation, in the application provided by the present invention, the mixing ratio of the roasted sample in the M32.5 cement is 19.5%.
[0029] As an optional implementation, in the resource recovery method provided by the present invention, the mixing ratio of the roasted sample in the M42.5 cement is 14.5%.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention adopts a method for roasting beryllium-containing silicon slag and a reducing coal auxiliary material, and the content of leached toxic beryllium in the obtained roasted sample is less than 0.02 mg / L. The obtained roasted sample can also be used as an admixture for cement clinker, so that the beryllium-containing silicon slag is disposed of as a resource. The roasting disposal process adopted in the present invention is simple, with low equipment investment, low operating cost, good curing effect of the roasted product, and no secondary pollution, which meets the requirements of safe, efficient and green disposal of beryllium-containing silicon slag. DETAILED DESCRIPTION
[0032] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in combination with the contents of the specification and preferred embodiments, but the protection scope of the present invention is not limited to the following specific embodiments.
[0033] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0035] Example 1
[0036] The resource disposal method of beryllium-containing silicon slag is as follows:
[0037] (1) Add auxiliary materials
[0038] The beryllium silicon slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its chemical composition is 0.13% Be, 11.54% S, 39.96% SiO2 and 15.62% CaO by weight. The moisture content of the beryllium silicon slag is 34.00%. The auxiliary material is reducing coal, which has 56.40% fixed carbon, 0.88% S, 14.88% moisture and 4893 kcal / kg calorific value.
[0039] According to the weight ratio of the auxiliary material added to the beryllium silicon-containing slag being 4%, the beryllium silicon-containing slag and the auxiliary material coal are evenly mixed to obtain the beryllium silicon-containing slag containing the auxiliary material.
[0040] (2) Calcination
[0041] The beryllium-containing silicon slag obtained in step (1) and the auxiliary material mixture were calcined at 950° C. for 30 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of the product obtained by this method was 0.00225 mg / L, which was lower than the standard of 0.02 mg / L.
[0042] Example 2
[0043] The resource disposal method of beryllium-containing silicon slag is as follows:
[0044] (1) Add auxiliary materials
[0045] The beryllium silicon slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its chemical composition is 0.12% Be, 12.75% S, 40.33% SiO2 and 14.55% CaO by weight. The moisture content of the beryllium silicon slag is 35.18%. The auxiliary material is reducing coal, which has 56.58% fixed carbon, 0.85% S, 15.31% moisture and 4599 kcal / kg calorific value.
[0046] According to the weight ratio of the auxiliary material added to the beryllium silicon-containing slag being 12%, the beryllium silicon-containing slag and the auxiliary material coal are evenly mixed to obtain the beryllium silicon-containing slag containing the auxiliary material.
[0047] (2) Calcination
[0048] The beryllium-containing silicon slag obtained in step (1) and the auxiliary material mixture were calcined at 950° C. for 45 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of the product obtained by this method was 0.00139 mg / L, which was lower than the standard of 0.02 mg / L.
[0049] Example 3
[0050] The resource disposal method of beryllium-containing silicon slag is as follows:
[0051] (1) Add auxiliary materials
[0052] The beryllium silicon slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its chemical composition is 0.13% Be, 11.12% S, 38.71% SiO2 and 16.22% CaO by weight. The moisture content of the beryllium silicon slag is 33.85%. The auxiliary materials contain 57.33% fixed carbon, 0.81% S, 15.85% water and 4795 kcal / kg calorific value.
[0053] According to the weight ratio of the auxiliary material added to the beryllium silicon-containing slag being 8%, the beryllium silicon-containing slag and the auxiliary material coal are evenly mixed to obtain the beryllium silicon-containing slag containing the auxiliary material.
[0054] (2) Calcination
[0055] The beryllium-containing silicon slag obtained in step (1) and the auxiliary material mixture were calcined at 1050° C. for 60 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of the product obtained by this method was 0.00099 mg / L, which was lower than the standard of 0.02 mg / L.
[0056] Example 4
[0057] The resource disposal method of beryllium-containing silicon slag is as follows:
[0058] (1) Add auxiliary materials
[0059] The beryllium silicon slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its components are analyzed. Its chemical composition is 0.15% Be, 12.09% S, 39.55% SiO2 and 15.11% CaO by weight, and the moisture content of the beryllium silicon slag is 33.27%. The fixed carbon in the auxiliary materials is 56.19%, S is 0.91%, the moisture is 14.68%, and the calorific value is 4632kcal / kg.
[0060] According to the weight ratio of the auxiliary material added to the beryllium silicon-containing slag being 6%, the beryllium silicon-containing slag and the auxiliary material coal are evenly mixed to obtain the beryllium silicon-containing slag containing the auxiliary material.
[0061] (2) Calcination
[0062] The beryllium-containing silicon slag obtained in step (1) and the auxiliary material mixture were calcined at 900° C. for 30 min using an exhaust-type high-temperature chamber muffle furnace to obtain a calcined sample. The leaching toxicity of the product obtained by this method was 0.00667 mg / L, which was lower than the standard of 0.02 mg / L.
[0063] Example 5
[0064] The resource disposal method of beryllium-containing silicon slag is as follows:
[0065] (1) Add auxiliary materials
[0066] The beryllium silicon slag in this embodiment is obtained by Minmetals Beryllium Industry Co., Ltd., and its chemical composition is 0.16% Be, 11.28% S, 41.55% SiO2 and 16.98% CaO by weight. The moisture content of the beryllium silicon slag is 35.97%. The fixed carbon in the auxiliary material is 58.36%, S is 0.81%, the moisture is 13.96%, and the calorific value is 4823kcal / kg.
[0067] According to the weight ratio of the auxiliary material added to the beryllium silicon-containing slag being 12%, the beryllium silicon-containing slag and the auxiliary material coal are evenly mixed to obtain the beryllium silicon-containing slag containing the auxiliary material.
[0068] (2) Calcination
[0069] The beryllium-containing silicon slag obtained in step (1) and the auxiliary material mixture were calcined at 1100° C. for 45 min using an exhaust-type high-temperature box muffle furnace to obtain a calcined sample. The leaching toxicity of the product obtained by this method was 0.0023 mg / L Be, which was lower than the standard of 0.02 mg / L.
[0070] Comparative Example 1
[0071] The resource disposal method of beryllium-containing silicon slag is as follows:
[0072] A. Ingredients
[0073] The beryllium-containing silicon slag of Example 1 was used. The beryllium-containing silicon slag was directly loaded into a corundum crucible without adding any auxiliary materials.
[0074] B. Roasting
[0075] The beryllium-containing silicon slag obtained in step A was calcined at 950° C. for 30 min using an exhaust-type high-temperature box muffle furnace. The obtained product was analyzed. The leaching toxicity of the product obtained by this method was 0.91 mg / L Be, which was higher than the standard of 0.02 mg / L.
[0076] Comparative Example 2
[0077] The resource disposal method of beryllium-containing silicon slag is as follows:
[0078] A. Ingredients
[0079] The beryllium-containing silicon slag of Example 2 was used. The beryllium-containing silicon slag was directly loaded into a corundum crucible without adding any auxiliary materials.
[0080] B. Roasting
[0081] The beryllium-containing silicon slag obtained in step A was calcined at 950° C. for 45 min using an exhaust-type high-temperature box muffle furnace. The obtained product was analyzed. The leaching toxicity of the product obtained by this method was 2.14 mg / L Be, which was higher than the standard of 0.02 mg / L.
[0082] Comparative Example 3
[0083] The resource disposal method of beryllium-containing silicon slag is as follows:
[0084] A. Ingredients
[0085] The beryllium-containing silicon slag of Example 3 was used. The beryllium-containing silicon slag was directly loaded into a corundum crucible without adding any auxiliary materials.
[0086] B. Roasting
[0087] The beryllium-containing silicon slag obtained in step A was calcined at 1050° C. for 60 min using an exhaust-type high-temperature box muffle furnace. The obtained product was analyzed. The leaching toxicity of the product obtained by this method was 0.105 mg / L Be, which was higher than the standard of 0.02 mg / L.
[0088] The calcined product obtained in Example 1 was subjected to phase analysis, and the phase composition was obtained according to the acid-base solution chemical analysis with different strengths. The results are shown in Appendix 1.
[0089] Table 1: Phase analysis of beryllium in calcined product in Example 1 / %
[0090] Phase Beryllium in Beryl Beryllium in Beryllium Sulfate Beryllium in Beryllium Silicate Total Beryllium content 0.09 0.0002 0.06 0.15 Distribution rate 60.00 0.13 39.87 100
[0091] It can be seen from Table 1 that after the beryllium-containing silicon slag is roasted with auxiliary coal, the basic phase composition of beryllium in the product is beryl, beryllium sulfate, and beryllium silicate, and the beryllium in the product mainly exists in the form of beryl.
[0092] The calcined product obtained in Example 1 is used as cement clinker admixture. The auxiliary material ratio and performance analysis are shown in Table 2.
[0093] Table 2: Performance test and analysis results of the calcined product used as cement clinker admixture in Example 1
[0094]
[0095] It can be seen from Table 2 that the proportion of the calcined sample prepared in Example 1 in the M32.5 type of cement can reach 19.5%, and the proportion in the M42.5 type of cement can reach 14.5%, and the setting time and compressive and flexural strengths of the cement all meet the requirements.
[0096] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for recycling beryllium-containing silicon slag. It is characterized in that The treatment method comprises the following steps: uniformly mixing beryllium-containing silicon slag and auxiliary materials, and then roasting them at 850°C to 1300°C to obtain a roasted sample; the auxiliary material is a reducing coal, wherein the fixed carbon content is greater than 55% and the calorific value is greater than 4000 kcal / kg; the amount of the auxiliary material added is 4 to 12% of the mass of the beryllium-containing silicon slag; The beryllium-containing silicon slag is obtained by mixing beryllium ore with concentrated sulfuric acid after smelting in the beryllium oxide production process, and reacting at 250-300° C. without reacting with sulfuric acid. The content of leached toxic beryllium in the roasted sample is less than 0.00667 mg / L, and the beryllium phase in the roasted sample is mainly beryl.
2. The resource disposal method of beryllium-containing silicon slag according to claim 1, It is characterized in that The beryllium-containing silicon slag has, by weight percentage, a beryllium content of less than 0.2%, a sulfur content of less than 15%, a silicon dioxide content of greater than 30%, and a calcium oxide content of greater than 10%.
3. The resource disposal method of beryllium-containing silicon slag according to claim 1, It is characterized in that The moisture content of the beryllium-containing silicon slag is 30% to 40%.
4. The method for recycling beryllium-containing silicon slag according to claim 1, It is characterized in that The beryllium-containing silicon slag and auxiliary materials are roasted in a muffle furnace, and the power of the muffle furnace is 10kW-20kW.
5. The resource disposal method of beryllium-containing silicon slag according to claim 1, It is characterized in that The calcination time is 30 to 60 minutes.
6. Application of the resource disposal method of beryllium-containing silicon slag according to any one of claims 1 to 5 in the preparation of cement clinker admixtures, It is characterized in that The calcined sample obtained after treatment is used to prepare cement clinker admixture.
7. The use according to claim 6, It is characterized in that The maximum amount of the roasted sample added to M32.5 cement is 19.5%, and the maximum amount of the roasted sample added to M42.5 cement is 14.5%.