A calcium carbonate cement, a hardened calcium carbonate cement body and its applications

By using materials such as vaterite and aragonite whiskers as crystal form regulators in calcium carbonate cement, it is prepared by carbonization and precipitation methods, and the rapid hardening and high compressive strength of calcium carbonate cement are achieved, and hardening in the existing technology is solved The problems of slow speed and insufficient compressive strength are suitable for low-carbon building materials.

CN116282997BActive Publication Date: 2024-11-12WUHAN UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310182489.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-11-12
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

The hardening speed of existing calcium carbonate cement is slow and the compressive strength is insufficient. The regulation method is single and the preparation method is limited, making it difficult to meet the needs of rapid hardening and high compressive strength.

Method used

The calcium carbonate cement precursor is vaterite or amorphous calcium carbonate, and aragonite whiskers, coral sand or shell powder are added as crystal form regulators. The amorphous calcium carbonate and vaterite are prepared by carbonization or precipitation method, and combined with crystal cores. Induction technology controls the crystal form transformation of calcium carbonate cement and forms an efficient hardened body.

Benefits of technology

It has achieved rapid hardening and high compressive strength of calcium carbonate cement, reaching 10-40MPa within one day of hardening, with a wide range of raw materials and low cost, and is suitable for the field of low-carbon building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116282997B_ABST
    Figure CN116282997B_ABST
Patent Text Reader

Abstract

The present invention discloses a calcium carbonate cement, a calcium carbonate cement hardener and its application, wherein the calcium carbonate cement comprises the following solid raw materials by mass: 30 to 100 parts of a calcium carbonate cement precursor, and 5 to 80 parts of a crystal form regulator; the calcium carbonate cement precursor is vaterite, or vaterite and amorphous calcium carbonate; the crystal form regulator comprises at least one of aragonite whiskers, coral sand or shell powder. The present invention controls the conversion of the calcium carbonate cement precursor to the target mineral aragonite by adding aragonite mineral materials such as aragonite whiskers, coral sand or shell powder as a crystal form regulator, and the aragonite can overlap in three-dimensional space to form a hardened body structure, thereby improving the compressive strength. The calcium carbonate cement of the present invention has a fast hardening speed, high compressive strength, and a wide range of raw material sources and low cost, and its hardening method is also simple and easy, so it has a wide range of applications in the field of building materials, especially in the field of low-carbon building materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inorganic non-metallic materials, and in particular relates to a calcium carbonate cement, a calcium carbonate cement hardener and applications thereof. Background Art

[0002] For every ton of Portland cement produced, the carbon emissions caused by the decomposition of calcium raw materials are about 500-550 kg / t, accounting for more than 58% of the total emissions of Portland cement. Low-carbon cement production is an important direction both at home and abroad, both within and outside the industry.

[0003] Calcium carbonate has its own "carbon cycle" characteristics in nature: that is, after calcium carbonate decomposes to generate CaO and emits CO2, it regenerates into calcium carbonate under environmental and chemical effects. Developing new cementitious material design and preparation technology with calcium carbonate as the cementing component is one of the important ways to solve the current carbon emission dilemma in the cement industry. Calcium carbonate, as an inorganic mineral widely existing in nature, has a variety of crystal forms. The crystal forms involved in the calcium carbonate cement system are mainly amorphous calcium carbonate, vaterite, aragonite and calcite, and the thermodynamic stability increases in turn. The hardened body formed by calcium carbonate crystals through grain boundaries, intermolecular interactions, etc. under the action of pressure, temperature or organic matter-induced templates has certain mechanical properties. Organisms use mineralization strategies to mineralize part of the tissue to form internal skeletons or external armor with superior hardness and toughness.

[0004] Calcium carbonate cement is a new type of cementitious material that forms bonding force based on the reconstruction and transformation of calcium carbonate phases. Hardening is inseparable from the transformation of calcium carbonate crystal forms. The key lies in the regulation of the calcium carbonate phase. The current methods for regulating the calcium carbonate phase are mainly through the addition of inorganic or organic additives to affect the lattice or crystal plane of calcium carbonate, control its nucleation growth, and regulate the phase and morphology.

[0005] At present, inorganic ions are mainly used as crystal modifiers in the preparation of calcium carbonate cement. 2+ As a crystal modifier, the coagulation and hardening process was completed in two hours, and the coagulation and hardening reached 6MPa. On this basis, Sr was added 2+ The material is prepared by pressure molding and cured for 3 to 7 days to solidify. It can be seen that the current control method is single and the preparation method is limited, and there is still room for improvement. Summary of the invention

[0006] In order to overcome the problems existing in the prior art, one of the objects of the present invention is to provide a calcium carbonate cement which can harden quickly and has high compressive strength.

[0007] A second object of the present invention is to provide a calcium carbonate cement hardened body comprising the above-mentioned calcium carbonate cement.

[0008] A third object of the present invention is to provide a method for preparing the above-mentioned calcium carbonate cement hardener.

[0009] A fourth object of the present invention is to provide an application of the above-mentioned calcium carbonate cement and calcium carbonate cement hardener.

[0010] In order to achieve the above object, the technical solution adopted by the present invention is:

[0011] The first aspect of the present invention provides a calcium carbonate cement, comprising the following solid raw materials in parts by weight: 30 to 100 parts of a calcium carbonate cement precursor and 5 to 80 parts of a crystal modifier; the calcium carbonate cement precursor is vaterite, or vaterite and amorphous calcium carbonate; the crystal modifier comprises at least one of aragonite whiskers, coral sand or shell powder.

[0012] There are many preparation methods for amorphous calcium carbonate, such as the decomposition of ammonium carbonate to produce CO2 and amorphous calcium carbonate, precipitation method (also known as double decomposition method), carbonization method, etc. Amorphous calcium carbonate can be obtained from various sources.

[0013] Among them, the carbonization method of amorphous calcium carbonate is a method for preparing amorphous calcium carbonate by diffusing gaseous CO2 into a calcium ion solution such as a calcium salt or calcium hydroxide solution. The calcium source can be derived from calcium-containing waste resources such as carbide slag, phosphogypsum, and construction solid waste, but is not limited to chemical reagents. CO2 comes from industrial waste gas, which can achieve resource recycling and reduce carbon emissions. It has the advantages of simple operation, abundant raw materials, and easy industrial production.

[0014] In a preferred embodiment of the present invention, amorphous calcium carbonate is prepared by a carbonization method.

[0015] Preferably, in the calcium carbonate cement, amorphous calcium carbonate is prepared by reacting CO2 and a calcium ion solution.

[0016] Preferably, in the calcium carbonate cement, the amorphous calcium carbonate is prepared by a method comprising the following steps: passing CO2 into a calcium ion solution, adding a stabilizer, carbonizing the solution until the pH value is 7 to 9, and separating and drying the precipitate generated by the reaction to obtain the amorphous calcium carbonate.

[0017] Preferably, the flow rate of CO2 is 400-600 mL / min; further preferably, the flow rate of CO2 is 450-550 mL / min; further preferably, the flow rate of CO2 is 500 mL / min.

[0018] Preferably, the calcium ion solution comprises at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate, a hydrate of calcium acetate or calcium hydroxide; further preferably, the calcium ion solution comprises at least one of a hydrate of calcium chloride, a hydrate of calcium nitrate or a hydrate of calcium acetate; further preferably, the calcium ion solution is selected from calcium chloride dihydrate.

[0019] Preferably, the concentration of the calcium ion solution is 0.8 to 1.2 mol / L; further preferably, the concentration of the calcium ion solution is 0.9 to 1.1 mol / L; preferably, the concentration of the calcium ion solution is 1 mol / L.

[0020] Preferably, the stabilizer includes at least one of magnesium ions, silicate ions, and phosphate ions; further preferably, the stabilizer is selected from magnesium ions; further preferably, the stabilizer is selected from anhydrous magnesium chloride.

[0021] Preferably, the concentration of the stabilizer is 0.08-0.12 mol / L; further preferably, the concentration of the stabilizer is 0.09-0.11 mol / L; further preferably, the concentration of the stabilizer is 0.1 mol / L.

[0022] Preferably, the carbonization reaction is performed until the pH value of the solution is 7.2 to 8.8; further preferably, the carbonization reaction is performed until the pH value of the solution is 7.5 to 8.5; further preferably, the carbonization reaction is performed until the pH value of the solution is 8.

[0023] In another preferred embodiment of the present invention, amorphous calcium carbonate is prepared by a precipitation method.

[0024] Preferably, in the calcium carbonate cement, amorphous calcium carbonate is prepared by reacting a calcium ion solution with a carbonate.

[0025] Preferably, in the calcium carbonate cement, the amorphous calcium carbonate is prepared by a method comprising the following steps: mixing 0.8-1.2 mol / L of a calcium ion solution with 0.08-0.12 mol / L of a carbonate in a volume ratio of 1:(7-11), and then separating and drying the precipitate generated by the reaction to obtain the amorphous calcium carbonate.

[0026] Preferably, in the preparation method of amorphous calcium carbonate, the calcium ion solution includes at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate, a hydrate of calcium acetate or calcium hydroxide; further preferably, in the preparation method of amorphous calcium carbonate, the calcium ion solution includes at least one of anhydrous calcium chloride, anhydrous calcium nitrate or anhydrous calcium acetate; further preferably, in the preparation method of amorphous calcium carbonate, the calcium ion solution is selected from anhydrous calcium chloride.

[0027] Preferably, in the preparation method of the amorphous calcium carbonate, the carbonate includes at least one of anhydrous sodium carbonate, a hydrate of sodium carbonate, anhydrous sodium bicarbonate, a hydrate of sodium bicarbonate, anhydrous potassium carbonate, a hydrate of potassium carbonate, anhydrous potassium bicarbonate, a hydrate of potassium bicarbonate, anhydrous ammonium carbonate, a hydrate of ammonium carbonate, anhydrous ammonium bicarbonate or a hydrate of ammonium bicarbonate; further preferably, in the preparation method of the amorphous calcium carbonate, the carbonate includes at least one of anhydrous sodium carbonate, anhydrous sodium bicarbonate, anhydrous potassium carbonate, anhydrous potassium bicarbonate, anhydrous ammonium carbonate or anhydrous ammonium bicarbonate; further preferably, in the preparation method of the amorphous calcium carbonate, the carbonate is selected from anhydrous sodium carbonate.

[0028] Preferably, in the method for preparing amorphous calcium carbonate, the concentration of the calcium ion solution is 0.85 to 1.15 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of the calcium ion solution is 0.9 to 1.1 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of the calcium ion solution is 0.95 to 1.05 mol / L.

[0029] Preferably, in the method for preparing amorphous calcium carbonate, the concentration of carbonate is 0.085-0.115 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of carbonate is 0.09-0.11 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of carbonate is 0.095-0.105 mol / L.

[0030] Preferably, in the method for preparing amorphous calcium carbonate, the volume ratio of calcium ion solution to carbonate is 1:(7.5-10.5); further preferably, in the method for preparing amorphous calcium carbonate, the volume ratio of calcium ion solution to carbonate is 1:(8-10); further preferably, in the method for preparing amorphous calcium carbonate, the volume ratio of calcium ion solution to carbonate is 1:(8.5-9.5).

[0031] Preferably, in the method for preparing amorphous calcium carbonate, the separation includes at least one of filtration, suction filtration or centrifugation; further preferably, in the method for preparing amorphous calcium carbonate, the separation includes at least one of filtration or suction filtration; even further preferably, in the method for preparing amorphous calcium carbonate, the separation is selected from suction filtration.

[0032] Preferably, in the method for preparing amorphous calcium carbonate, the drying temperature is 40 to 80°C; further preferably, in the method for preparing amorphous calcium carbonate, the drying temperature is 50 to 70°C; further preferably, in the method for preparing amorphous calcium carbonate, the drying temperature is 55 to 65°C.

[0033] Preferably, in the method for preparing amorphous calcium carbonate, the drying time is 12 to 36 hours; further preferably, in the method for preparing amorphous calcium carbonate, the drying time is 18 to 30 hours; further preferably, in the method for preparing amorphous calcium carbonate, the drying time is 22 to 26 hours.

[0034] Preferably, in the preparation method of amorphous calcium carbonate, the precipitate is washed after separation and before drying; further preferably, the washing solvent includes at least one of water and an organic solvent; further preferably, the washing solvent is deionized water and anhydrous ethanol.

[0035] Preferably, the purity of amorphous calcium carbonate in the calcium carbonate cement is 90-100%; further preferably, the purity of amorphous calcium carbonate in the calcium carbonate cement is 94-100%; further preferably, the purity of amorphous calcium carbonate in the calcium carbonate cement is 98-100%.

[0036] There are also many preparation methods for vaterite, such as thermal decomposition, precipitation, carbonization, etc. It can be seen that there are many sources for obtaining vaterite.

[0037] Among them, the carbonization method of vaterite is similar to the carbonization method of amorphous calcium carbonate. Both involve diffusing gaseous CO2 into a calcium ion solution such as a calcium salt or calcium hydroxide solution for reaction, but the specific experimental conditions are different. The calcium ion-containing solution can also come from waste resources such as carbide slag, phosphogypsum, and construction solid waste, and is not limited to chemical reagents. CO2 can also come from industrial waste gas, which can achieve resource recycling and reduce carbon emissions. It also has the advantages of simple operation, abundant raw materials, and easy industrial production.

[0038] In a preferred embodiment of the present invention, vaterite is prepared by carbonization method.

[0039] Preferably, in the calcium carbonate cement, vaterite is prepared by reacting CO2, aqueous ammonia and calcium ion solution.

[0040] Preferably, in the calcium carbonate cement, vaterite is prepared by a method comprising the following steps: adding ammonia water to a calcium ion solution, introducing CO2 until the pH of the solution is 7 to 9, and separating and drying the precipitate generated by the reaction to obtain the vaterite.

[0041] Preferably, the calcium ion solution includes at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate, a hydrate of calcium acetate or calcium hydroxide; further preferably, the calcium ion solution includes at least one of anhydrous calcium chloride, anhydrous calcium nitrate or anhydrous calcium acetate; further preferably, the calcium ion solution is selected from anhydrous calcium chloride.

[0042] Preferably, the concentration of the calcium ion solution is 0.1-0.2 mol / L; further preferably, the concentration of the calcium ion solution is 0.12-0.18 mol / L; preferably, the concentration of the calcium ion solution is 0.15 mol / L.

[0043] Preferably, the concentration of the ammonia water is 25-28 wt %; further preferably, the concentration of the ammonia water is 26-27 wt %; further preferably, the concentration of the ammonia water is 26 wt %.

[0044] Preferably, the amount of ammonia water added is 1-6% of the volume of the calcium ion solution; further preferably, the amount of ammonia water added is 2-5% of the volume of the calcium ion solution; further preferably, the amount of ammonia water added is 3-4% of the volume of the calcium ion solution.

[0045] Preferably, the flow rate of CO2 is 500-700 mL / min; further preferably, the flow rate of CO2 is 550-650 mL / min; further preferably, the flow rate of CO2 is 600 mL / min.

[0046] Preferably, CO2 is introduced until the pH of the solution is 7.2-8.8; further preferably, CO2 is introduced until the pH of the solution is 7.5-8.5; further preferably, CO2 is introduced until the pH of the solution is 8.

[0047] In another preferred embodiment of the present invention, vaterite is prepared by a precipitation method. Preferably, in the calcium carbonate cement, vaterite is prepared by the reaction of a calcium ion solution and a carbonate.

[0048] Preferably, in the calcium carbonate cement, vaterite is prepared by a method comprising the following steps: mixing 1.8-2.2 mol / L of calcium ion solution and 1.8-2.2 mol / L of carbonate in an equal volume ratio, and then separating and drying the precipitate generated by the reaction to obtain the vaterite.

[0049] Preferably, in the method for preparing vaterite, the calcium ion solution includes at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate or a hydrate of calcium acetate; further preferably, in the method for preparing vaterite, the calcium ion solution includes at least one of a hydrate of calcium chloride, a hydrate of calcium nitrate or a hydrate of calcium acetate; further preferably, in the method for preparing vaterite, the calcium ion solution is selected from calcium chloride dihydrate.

[0050] Preferably, in the preparation method of vaterite, the carbonate includes at least one of anhydrous sodium carbonate, a hydrate of sodium carbonate, anhydrous sodium bicarbonate, a hydrate of sodium bicarbonate, anhydrous potassium carbonate, a hydrate of potassium carbonate, anhydrous potassium bicarbonate, a hydrate of potassium bicarbonate, anhydrous ammonium carbonate, a hydrate of ammonium carbonate, anhydrous ammonium bicarbonate or a hydrate of ammonium bicarbonate; further preferably, in the preparation method of vaterite, the carbonate includes at least one of anhydrous sodium carbonate, anhydrous sodium bicarbonate, anhydrous potassium carbonate, anhydrous potassium bicarbonate, anhydrous ammonium carbonate or anhydrous ammonium bicarbonate; further preferably, in the preparation method of vaterite, the carbonate is selected from anhydrous potassium carbonate.

[0051] Preferably, in the method for preparing vaterite, the concentration of the calcium ion solution is 1.85 to 2.15 mol / L; further preferably, in the method for preparing vaterite, the concentration of the calcium ion solution is 1.9 to 2.1 mol / L; further preferably, in the method for preparing vaterite, the concentration of the calcium ion solution is 1.95 to 2.05 mol / L.

[0052] Preferably, in the method for preparing vaterite, the concentration of carbonate is 1.85 to 2.15 mol / L; further preferably, in the method for preparing vaterite, the concentration of carbonate is 1.9 to 2.1 mol / L; further preferably, in the method for preparing vaterite, the concentration of carbonate is 1.95 to 2.05 mol / L.

[0053] Preferably, in the method for preparing vaterite, the separation includes at least one of filtration, suction filtration or centrifugation; further preferably, in the method for preparing vaterite, the separation includes at least one of filtration or suction filtration; even further preferably, in the method for preparing vaterite, the separation is selected from suction filtration.

[0054] Preferably, in the method for preparing vaterite, the drying temperature is 40 to 80°C; further preferably, in the method for preparing vaterite, the drying temperature is 50 to 70°C; further preferably, in the method for preparing vaterite, the drying temperature is 55 to 65°C.

[0055] Preferably, in the method for preparing vaterite, the drying time is 12 to 36 hours; further preferably, in the method for preparing vaterite, the drying time is 18 to 30 hours; further preferably, in the method for preparing vaterite, the drying time is 22 to 26 hours.

[0056] Preferably, in the method for preparing vaterite, the precipitate is washed after being separated and before being dried; further preferably, the washing solvent includes at least one of water and an organic solvent; further preferably, the washing solvent is deionized water and anhydrous ethanol.

[0057] Preferably, in the calcium carbonate cement, the purity of vaterite is 90-100%; further preferably, in the calcium carbonate cement, the purity of vaterite is 92-100%; further preferably, in the calcium carbonate cement, the purity of vaterite is 95-100%.

[0058] Preferably, in the calcium carbonate cement, when the calcium carbonate cement precursors are vaterite and amorphous calcium carbonate, the mass ratio of amorphous calcium carbonate to vaterite is (0.25-1):1; further preferably, in the calcium carbonate cement, when the calcium carbonate cement precursors are vaterite and amorphous calcium carbonate, the mass ratio of amorphous calcium carbonate to vaterite is (0.3-0.8):1; further preferably, in the calcium carbonate cement, when the calcium carbonate cement precursors are vaterite and amorphous calcium carbonate, the mass ratio of amorphous calcium carbonate to vaterite is (0.3-0.6):1.

[0059] Preferably, in the calcium carbonate cement and the crystal form regulator, the average aspect ratio of the aragonite whiskers is 5 to 40; further preferably, in the calcium carbonate cement and the crystal form regulator, the average aspect ratio of the aragonite whiskers is 7 to 20; further preferably, in the calcium carbonate cement and the crystal form regulator, the average aspect ratio of the aragonite whiskers is 8 to 12.

[0060] Preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of the aragonite whiskers is 85 to 100 wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of the aragonite whiskers is 90 to 100 wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of the aragonite whiskers is 98 to 100 wt%.

[0061] Preferably, in the calcium carbonate cement and the crystal form regulator, the average particle size of the coral sand is 20 to 300 μm; further preferably, in the calcium carbonate cement and the crystal form regulator, the average particle size of the coral sand is 40 to 150 μm; further preferably, in the calcium carbonate cement and the crystal form regulator, the average particle size of the coral sand is 60 to 100 μm.

[0062] Preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of coral sand is 75-100wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of coral sand is 90-98wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of coral sand is 95-97wt%.

[0063] Preferably, in the calcium carbonate cement, in the crystal form regulator, the average particle size of the shell powder is 25 to 300 μm; further preferably, in the calcium carbonate cement, in the crystal form regulator, the average particle size of the shell powder is 30 to 200 μm; further preferably, in the calcium carbonate cement, in the crystal form regulator, the average particle size of the shell powder is 40 to 70 μm.

[0064] Preferably, in the calcium carbonate cement, the aragonite content of shell powder in the crystal form regulator is 70-100wt%; further preferably, in the calcium carbonate cement, the aragonite content of shell powder in the crystal form regulator is 85-95wt%; further preferably, in the calcium carbonate cement, the aragonite content of shell powder in the crystal form regulator is 92-94wt%.

[0065] Preferably, the raw materials of the calcium carbonate cement also include water; further preferably, the mass ratio of water to solid raw materials is 0.1-0.5; further preferably, the mass ratio of water to solid raw materials is 0.2-0.4; more preferably, the mass ratio of water to solid raw materials is 0.25-0.35.

[0066] Preferably, in the calcium carbonate cement, the mass fraction of the calcium carbonate cement precursor is 40 to 90 parts; further preferably, in the calcium carbonate cement, the mass fraction of the calcium carbonate cement precursor is 45 to 80 parts; further preferably, in the calcium carbonate cement, the mass fraction of the calcium carbonate cement precursor is 50 to 70 parts.

[0067] Preferably, in the calcium carbonate cement, the mass fraction of the crystal form regulator is 20 to 70 parts; further preferably, in the calcium carbonate cement, the mass fraction of the crystal form regulator is 25 to 60 parts; further preferably, in the calcium carbonate cement, the mass fraction of the crystal form regulator is 30 to 50 parts.

[0068] Preferably, the calcium carbonate cement comprises the following raw materials in parts by weight: 40 to 90 parts of calcium carbonate cement precursor and 20 to 70 parts of crystal modifier.

[0069] Further preferably, the calcium carbonate cement comprises the following raw materials in parts by weight: 45 to 80 parts of calcium carbonate cement precursor and 25 to 60 parts of crystal modifier.

[0070] More preferably, the calcium carbonate cement comprises the following raw materials in parts by weight: 50 to 70 parts of calcium carbonate cement precursor and 30 to 50 parts of crystal modifier.

[0071] The second aspect of the present invention provides a calcium carbonate cement hardened body formed by the calcium carbonate cement described in the first aspect of the present invention.

[0072] Preferably, the aragonite content of the hardened calcium carbonate cement body is 70 to 100 wt %; further preferably, the aragonite content of the hardened calcium carbonate cement body is 80 to 100 wt %; further preferably, the aragonite content of the hardened calcium carbonate cement body is 94 to 99 wt %.

[0073] Preferably, the porosity of the hardened calcium carbonate cement body is 20-60%; further preferably, the porosity of the hardened calcium carbonate cement body is 25-50%; further preferably, the porosity of the hardened calcium carbonate cement body is 30-40%.

[0074] The third aspect of the present invention provides a method for preparing the hardened calcium carbonate cement body according to the second aspect of the present invention, the preparation method comprising the following steps: mixing the raw materials of the calcium carbonate cement, and then molding and curing to obtain the hardened calcium carbonate cement body.

[0075] Preferably, in the preparation method, amorphous calcium carbonate and vaterite are first mixed to obtain a calcium carbonate cement precursor, and then a crystal modifier is added and mixed to obtain a solid raw material for calcium carbonate cement.

[0076] Preferably, in the preparation method, the mixing time of amorphous calcium carbonate and vaterite is 1 to 8 minutes; further preferably, in the preparation method, the mixing time of amorphous calcium carbonate and vaterite is 2 to 6 minutes; further preferably, in the preparation method, the mixing time of amorphous calcium carbonate and vaterite is 2 to 4 minutes.

[0077] Preferably, in the preparation method, the mixing time for adding the crystal form regulator for mixing is 2 to 10 minutes; further preferably, in the preparation method, the mixing time for adding the crystal form regulator for mixing is 3 to 8 minutes; further preferably, in the preparation method, the mixing time for adding the crystal form regulator for mixing is 4 to 6 minutes.

[0078] Preferably, in the preparation method, the molding includes at least one of extrusion molding, casting molding, and compression molding.

[0079] Preferably, in the preparation method, the molding pressure is 0 to 200 MPa; further preferably, in the preparation method, the molding pressure is 50 to 150 MPa; further preferably, in the preparation method, the molding pressure is 50 to 100 MPa.

[0080] Preferably, in the preparation method, the curing includes at least one of air curing, water curing or steam curing.

[0081] Preferably, in the preparation method, the curing time is 1 to 5 days; further preferably, in the preparation method, the curing time is 1 to 3 days; further preferably, in the preparation method, the curing time is 1 to 2 days.

[0082] Preferably, in the preparation method, the curing temperature is 20-120°C; further preferably, in the preparation method, the curing temperature is 30-110°C; further preferably, in the preparation method, the curing temperature is 40-100°C.

[0083] The fourth aspect of the present invention provides an application of the calcium carbonate cement described in the first aspect of the present invention, or the hardened calcium carbonate cement described in the second aspect of the present invention in the field of building materials.

[0084] Preferably, the field of building materials is the field of low-carbon building materials.

[0085] The beneficial effects of the present invention are:

[0086] The calcium carbonate cement of the present invention uses crystal transformation as the source of bonding force, and by adding aragonite mineral materials such as aragonite whiskers, coral sand or shell powder as crystal form regulators, the crystal form regulation is achieved by means of crystal nucleus induction, and the calcium carbonate cement precursor is controlled to be transformed into the target mineral aragonite. Aragonite can overlap in three-dimensional space to form a hardened body structure. The calcium carbonate cement of the present invention has a fast hardening speed and high compressive strength. A calcium carbonate cement hardened body with a compressive strength of 10 to 40 MPa can be obtained within 1 day of hardening. In the calcium carbonate cement precursor, amorphous calcium carbonate and vaterite are both thermodynamically unstable calcium carbonate crystal forms, and can be converted into rod-shaped aragonite through the regulation of the crystal form regulator. Among them, amorphous calcium carbonate has higher activity and is easier to be converted into aragonite than vaterite, which is conducive to the reaction process, but has little effect on mechanical properties. Aragonite whiskers have been industrially produced as modified materials, and aragonite mineral materials such as coral sand and shell powder can be used in the field of marine engineering islands and reefs according to local conditions. The calcium carbonate cement of the present invention has a wide range of raw materials, low cost, and its hardening method is also simple and easy. Therefore, it has a wide range of applications in the field of building materials, especially in the field of low-carbon building materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0087] Figure 1 1 is the XRD diagram of amorphous calcium carbonate and vaterite in the examples and comparative examples.

[0088] Figure 2 1 is the XRD diagram of the hardened calcium carbonate cement of Examples 1 to 4 and Comparative Example 1.

[0089] Figure 3 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 1.

[0090] Figure 4 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 2.

[0091] Figure 5 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 3.

[0092] Figure 6 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 4.

[0093] Figure 7 This is the SEM image of the hardened calcium carbonate cement body of Comparative Example 1 cured for 1 day.

[0094] Figure 8 This is the SEM image of the hardened calcium carbonate cement body of Comparative Example 2 cured for 1 day. DETAILED DESCRIPTION

[0095] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.

[0096] The amorphous calcium carbonate and vaterite used in the examples and comparative examples of the present invention are both prepared by precipitation method.

[0097] The preparation method of amorphous calcium carbonate is as follows: 1 mol / L anhydrous calcium chloride and 0.1 mol / L sodium carbonate are mixed in a volume ratio of 1:9, the precipitate is immediately filtered, the filter cake is washed with deionized water and anhydrous ethanol, and then dried at 60°C for 24 hours.

[0098] The preparation method of vaterite is as follows: after mixing 2.0 mol / L of equal volume and concentration of calcium chloride dihydrate and anhydrous potassium carbonate, the precipitate is filtered, the filter cake is washed with deionized water and anhydrous ethanol and then dried at 60° C. for 24 hours.

[0099] XRD was used to characterize the products of amorphous calcium carbonate and vaterite. The XRD patterns are shown in Figure 1 As shown, the purity of amorphous calcium carbonate is 100% and the purity of vaterite is 98%.

[0100] The average aspect ratio of the aragonite whiskers used in the embodiments of the present invention and the comparative examples is 10, and the aragonite content is 99wt%; the average particle size of the coral sand is 80μm, and the aragonite content is 97wt%; the average particle size of the shell powder is 50μm, and the aragonite content is 94wt%.

[0101] Example 1

[0102] A calcium carbonate cement comprises the following solid raw materials in parts by weight: 15 parts of amorphous calcium carbonate, 45 parts of vaterite, and 10 parts of aragonite whiskers.

[0103] The preparation method of the hardened calcium carbonate cement is as follows: amorphous calcium carbonate and vaterite are mixed in a stirring pot at a mass ratio of 1:3, and after stirring for 3 minutes, 40 parts of aragonite whiskers are added, and after stirring for 5 minutes, water is mixed with the solid raw material at a water-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and pressurized using an automatic press with a molding pressure of 100 MPa. After pressurization for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm. The test block is placed in a steam environment at a temperature of 60°C for curing to obtain a hardened calcium carbonate cement.

[0104] Example 2

[0105] A calcium carbonate cement comprises the following solid raw materials in parts by weight: 15 parts of amorphous calcium carbonate, 45 parts of vaterite, and 30 parts of coral sand.

[0106] The preparation method of the calcium carbonate cement hardener is as follows: amorphous calcium carbonate and vaterite are mixed in a stirring pot at a mass ratio of 1:3, and after stirring for 3 minutes, 40 parts of coral sand are added, and after stirring for 5 minutes, water is mixed with the solid raw material at a water-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and pressurized using an automatic press with a molding pressure of 100 MPa. After pressurization for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm. The test block is placed in a steam environment at a temperature of 80°C for curing to obtain a calcium carbonate cement hardener.

[0107] Example 3

[0108] A calcium carbonate cement comprises the following solid raw materials in parts by weight: 20 parts of amorphous calcium carbonate, 40 parts of vaterite, and 40 parts of shell powder.

[0109] The preparation method of the hardened calcium carbonate cement is as follows: amorphous calcium carbonate and vaterite are mixed in a stirring pot at a mass ratio of 1:2, and after stirring for 3 minutes, 40 parts of shell powder are added, and after stirring for 5 minutes, water is mixed with the solid raw material at a water-to-solid ratio of 0.30 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and an automatic press is used for pressurization, and the molding pressure is 100 MPa. After pressurization for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm. The test block is placed in a steam environment at a temperature of 40°C for curing to obtain a hardened calcium carbonate cement.

[0110] Example 4

[0111] A calcium carbonate cement comprises the following solid raw materials in parts by weight: 60 parts of vaterite and 60 parts of coral sand.

[0112] The preparation method of the hardened calcium carbonate cement is as follows: 60 parts of vaterite and 40 parts of coral sand are mixed in a stirring pot, and after stirring for 5 minutes, water is mixed with the solid raw material at a water-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and pressurized using an automatic press with a molding pressure of 50 MPa. After pressurizing for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm. The test block is placed in a steam environment at a temperature of 100°C for curing to obtain a hardened calcium carbonate cement.

[0113] Comparative Example 1

[0114] A calcium carbonate cement comprises the following solid raw materials in parts by weight: 20 parts of amorphous calcium carbonate, 60 parts of vaterite, and 20 parts of anhydrous magnesium chloride.

[0115] The preparation method of the hardened calcium carbonate cement is as follows: amorphous calcium carbonate and vaterite are mixed in a stirring pot at a mass ratio of 1:3, and after stirring for 3 minutes, 20 parts of anhydrous magnesium chloride are added, and after stirring for 5 minutes, water is mixed with the solid raw material at a water-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and pressurized using an automatic press with a molding pressure of 50 MPa. After pressurization for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm. The test block is placed in a steam environment at a temperature of 60°C for curing to obtain a hardened calcium carbonate cement.

[0116] Comparative Example 2

[0117] A calcium carbonate cement comprises the following solid raw materials in parts by weight: 20 parts of amorphous calcium carbonate and 40 parts of vaterite.

[0118] The preparation method of the hardened calcium carbonate cement is as follows: amorphous calcium carbonate and vaterite are mixed in a stirring pot at a mass ratio of 1:2, and after stirring for 3 minutes, water is mixed with the solid raw material at a water-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and pressurized using an automatic press with a molding pressure of 50 MPa. After pressurizing for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm. The test block is placed in a steam environment at a temperature of 60°C for curing to obtain a hardened calcium carbonate cement.

[0119] Performance Testing

[0120] 1) The compressive strength of the hardened calcium carbonate cement obtained in Examples 1 to 4 and Comparative Example 1 was tested using an electronic universal testing machine at a loading speed of 1 mm / min. The 1-day compressive strength is the compressive strength of the hardened calcium carbonate cement after curing for 1 day, and the 28-day compressive strength is the compressive strength of the hardened calcium carbonate cement after curing for 28 days.

[0121] 2) The setting time, aragonite content and porosity of the calcium carbonate cement hardened body obtained in Examples 1 to 4 and Comparative Example 1 were tested. The setting time is the curing time required for amorphous calcium carbonate and vaterite to be completely transformed into aragonite. XRD and infrared were used to measure the phase composition of calcium carbonate at different curing times. When the crystal transformation is completed, the curing is complete, and the curing time is the setting time; the aragonite content is obtained by quantitative analysis based on the XRD diagram; the porosity is obtained by mercury injection.

[0122] 3) XRD patterns and SEM patterns of the hardened calcium carbonate cement of test examples 1 to 4 and comparative example 1.

[0123] The test results are recorded in Table 1.

[0124] Table 1 Test results of Examples 1 to 4 and Comparative Example 1

[0125]

[0126]

[0127] The compressive strength of the hardened calcium carbonate cement obtained in Examples 1 to 4 is higher than that in Comparative Example 1. It can be seen that the present invention can better promote the conversion of calcium carbonate cement precursor to target mineral aragonite by adding aragonite whiskers, coral sand or shell powder as a crystal form regulator, compared with inorganic ions such as magnesium ions, and significantly improve the compressive strength of the hardened body structure formed by aragonite overlapping in three-dimensional space. Specifically, Figure 2 The XRD diagrams of the hardened calcium carbonate cements of Examples 1 to 4 and Comparative Examples 1 to 2 cured for 1 day show that the hardened bodies of Examples 1 to 4 and Comparative Example 1 are mainly aragonite phases, and the hardened body of Comparative Example 2 without adding a crystal form regulator is mainly calcite phase, indicating that anhydrous magnesium chloride and aragonite mineral materials such as aragonite whiskers, coral sand or shell powder of the present invention all have the effect of inducing aragonite formation. Figure 3 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 1. Figure 4 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 2. Figure 5 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 3. Figure 6 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 4. Figure 7This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Comparative Example 1. Figure 8 This is the SEM image of the hardened calcium carbonate cement of Comparative Example 2 cured for 1 day. The rhombohedral shape is a calcite structure, and the needle-rod shape is an aragonite structure. It can be seen from the figure that Figure 7 The aragonite structure formed in the embodiment is shorter and thicker, and arranged irregularly, so it is not conducive to forming an intertwined three-dimensional spatial structure. Its hardened body has poor bonding properties, high porosity, and low compressive strength. Compared with comparative example 1, embodiments 1 to 4 have a better effect of promoting the formation of needle-rod aragonite structure. The aragonite is more slender, which is more conducive to forming an intertwined three-dimensional spatial structure, thereby making the hardened body have higher compressive strength. Figure 8 It can be seen that the calcite formed by the conversion of comparative example 2 is a rhombohedron, which cannot form a lapped structure similar to aragonite, has poor bonding strength, and the hardened body formed has a large pore size and many pores, resulting in low strength. In addition, the compressive strength of the test block with a larger molding pressure is relatively high; appropriately increasing the curing temperature can accelerate the curing rate without affecting the strength.

[0128] The invention controls the conversion of a calcium carbonate cement precursor into a target mineral aragonite by adding aragonite whiskers, coral sand or shell powder and other aragonite mineral materials as a crystal form regulator. The aragonite can be overlapped in a three-dimensional space to form a hardened body structure, thereby improving the compressive strength. The calcium carbonate cement of the invention has a fast hardening speed and high compressive strength. A hardened calcium carbonate cement body with a compressive strength of 10 to 40 MPa can be obtained after hardening for one day. The raw material source is wide and the cost is low. The hardening method is also simple and easy. Therefore, the invention has a wide application in the field of building materials, especially in the field of low-carbon building materials.

Claims

1. A calcium carbonate cement, characterized in that The invention comprises the following solid raw materials in parts by mass: 30 to 100 parts of a calcium carbonate cement precursor and 5 to 80 parts of a crystal modifier; the calcium carbonate cement precursor is vaterite and amorphous calcium carbonate; the crystal modifier comprises at least one of aragonite whiskers, coral sand or shell powder; the mass ratio of the amorphous calcium carbonate to the vaterite is (0.25 to 1):

1.

2. The calcium carbonate cement according to claim 1, characterized in that The average aspect ratio of the aragonite whiskers is 5 to 40; and / or, the aragonite whiskers have an aragonite content of 85 to 100 wt %; And / or, the average particle size of the coral sand is 20 to 300 μm; And / or, the coral sand has an aragonite content of 75 to 100 wt%; And / or, the average particle size of the shell powder is 25 to 300 μm; And / or, the aragonite content of the shell powder is 70-100wt%.

3. The calcium carbonate cement according to any one of claims 1 to 2, characterized in that The raw materials of the calcium carbonate cement also include water; the mass ratio of the water to the solid raw materials is 0.1 to 0.

5.

4. A hardened calcium carbonate cement body, characterized in that: The calcium carbonate cement hardened body is formed by the calcium carbonate cement according to any one of claims 1 to 3.

5. The hardened calcium carbonate cement body according to claim 4, characterized in that: The aragonite content of the hardened calcium carbonate cement is 70-100wt%.

6. The hardened calcium carbonate cement body according to claim 4, characterized in that: The porosity of the hardened calcium carbonate cement body is 20-60%.

7. The method for preparing a hardened calcium carbonate cement body according to any one of claims 4 to 6, characterized in that: The following steps are involved: The various raw materials of calcium carbonate cement are mixed, and then molded and cured to obtain the calcium carbonate cement hardened body.

8. The preparation method according to claim 7, characterized in that: The molding pressure is 0 to 200 MPa; And / or, the curing time is 1 to 5 days; And / or, the curing temperature is 20-120°C.

9. Use of the calcium carbonate cement according to any one of claims 1 to 3, or the hardened calcium carbonate cement according to any one of claims 4 to 6 in the field of building materials.

Citation Information

Patent Citations

  • Methods and systems for utilizing carbide lime

    CN104487458A

  • Calcium carbonate-based sand powder reinforced carbonized hardened body and preparation method thereof

    CN113121192A

  • Calcium carbonate gel, preparation method and application

    CN114907036A

  • Micro rod-like aragonite type calcium carbonate and preparation method thereof

    CN115072757A

  • Acicular or columnar particle of calcium carbonate having high purity aragonite structure formed by carbon dioxide bubbling method, and method for manufacturing the same

    JP2008222533A