Polyethylene resin composition for bottle cap, preparation method thereof and molded product prepared therefrom

By combining antioxidant, neutralizing agent and slip-in enhancer, the flowability and hardening modulus of the polyethylene resin are optimized, and the existing polyethylene bottle cap material is solved in ultra-thin The limitations in the process of shaping and lightweighting achieve a combination of high flowability and high hardening modulus, which is suitable for molded products of bottle caps.

CN116285071BActive Publication Date: 2024-11-19HANWHA TOTALENERGIES PETROCHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211396210.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-12-21
Filing Date
2022-11-09
Publication Date
2024-11-19
Estimated Expiration
2042-11-09

AI Technical Summary

Technical Problem

During the ultra-thinning and lightweighting process, the existing polyethylene bottle cap materials have excellent fluidity and poor impact strength and strain hardening modulus, or excellent impact strength and strain hardening modulus and poor flowability, resulting in limitations during processing.

Method used

Using a polyethylene resin composition, the second stage polymerization of the polyethylene resin formed in the first and second reactors is carried out, combining antioxidant, neutralizing agent and slippage agent to optimize its zero shear viscosity and short branching. The number of chains, polymerization weight ratio and strain hardening modulus improve its fluidity, impact strength and strain hardening modulus.

Benefits of technology

The high flowability, impact strength and strain hardening modulus of the polyethylene resin composition during processing are achieved, and the lightweight and ultra-thinization of the bottle cap is easily achieved, which improves productivity and long-term storage stability and sealing of the molded product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005038977640000081
    Figure GDA0005038977640000081
  • Figure GDA0005038977640000091
    Figure GDA0005038977640000091
  • Figure GDA0005038977640000092
    Figure GDA0005038977640000092
Patent Text Reader

Abstract

The present invention relates to a polyethylene resin composition for bottle caps, a preparation method thereof and a molded product prepared therefrom. The polyethylene resin composition for bottle caps comprises a polyethylene resin formed by a first reactor and a second reactor, wherein the polyethylene resin formed in the first reactor has a zero shear viscosity of 10 based on an ARES rheometer at 180°C. 6 Moor ~ 10 7 Park, based on 13 The number of short chain branches per 1000 carbon atoms of C-NMR is 2.5-6.0, the zero shear viscosity ratio of the polyethylene resin formed in the first reactor to the polyethylene resin formed in the second reactor based on an ARES rheometer at 180°C is 11-20, the polymerization weight ratio of the polyethylene resin formed in the first reactor to the polyethylene resin formed in the second reactor is 40-60:40-60, and the strain hardening modulus is 20 MPa-30 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyethylene resin composition for bottle caps, a preparation method thereof and a molded product prepared therefrom. Background Art

[0002] Due to the diversification of packaging containers and the expansion of classified recycling for environmental reasons, the plasticization of bottle cap materials used in beverage containers such as glass bottles and polyethylene terephthalate (PET) is increasing.

[0003] Plastic bottle caps are mainly made of high-density polyethylene and polypropylene. Bottle caps based on these materials are lighter than existing aluminum bottle caps, are non-corrosive, and have excellent moldability and diverse molding designs, so their use is increasing. In particular, high-density polyethylene is softer than polypropylene, and unlike polypropylene bottle caps that require additional gaskets to seal the contents of beverage containers, high-density polyethylene has the advantage of being able to keep the contents sealed even without a gasket.

[0004] As the use of polyethylene as bottle caps continues to expand, bottle caps are being made ultra-thin and lightweight in order to reduce the amount of plastic used. Ultra-thin and lightweight require high fluidity, excellent impact strength and strain hardening modulus during processing. However, as for the original polyethylene material for bottle caps, it has excellent fluidity but poor impact strength and strain hardening modulus, or excellent impact strength and strain hardening modulus but poor fluidity, so there are limitations in ultra-thin and lightweight. Summary of the invention

[0005] Technical issues

[0006] One embodiment provides a polyethylene resin composition for bottle caps, which has excellent fluidity when processed into a molded product, high impact strength and strain hardening modulus, and multimodal properties that facilitate lightweighting and ultra-thinning.

[0007] Another implementation example provides a method for preparing the polyethylene resin composition for bottle caps.

[0008] Another implementation example provides a molded product prepared from the polyethylene resin composition for bottle caps.

[0009] Technical Solution

[0010] One embodiment provides a polyethylene resin composition for bottle caps, wherein the polyethylene resin is formed by a first reactor and a second reactor, wherein the polyethylene resin formed in the first reactor has a zero shear viscosity (η0 1st ) is 10 6 Moor ~ 107 Park, based on 13 The number of short chain branches per 1000 carbon atoms (SCB) of C-NMR 1st ) is 2.5 to 6.0, and the polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor have a zero shear viscosity ratio (η0 1st / η0 2nd ) is 11 to 20, the polymerization weight ratio of the polyethylene resin formed in the first reactor to the polyethylene resin formed in the second reactor is 40 to 60:40 to 60, and the strain hardening modulus is 20 MPa to 30 MPa.

[0011] The polyethylene resin composition may have a melt flow rate ratio (MFRR) of 80 to 180.

[0012] The density of the polyethylene resin composition can be 0.950 g / cm 3 ~0.965g / cm 3 .

[0013] The polyethylene resin composition may further include one or more selected from an antioxidant, a neutralizer and a slip agent.

[0014] The polyethylene resin composition may contain 0.01 to 0.5 parts by weight of the antioxidant relative to 100 parts by weight of the polyethylene resin composition. The antioxidant may be one or more selected from 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,6-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamido]hexane, 1,6-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamido]propane, tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol-di-phosphite and bis(2,4-di-tert-butylphenyl)pentaerythritol-di-phosphite.

[0015] The polyethylene resin composition may contain 0.01 to 0.3 parts by weight of the neutralizer relative to 100 parts by weight of the polyethylene resin composition. The neutralizer may include calcium stearate, zinc stearate, magnesium hydroxyaluminum carbonate, zinc oxide, magnesium hydroxystearate, or a combination thereof.

[0016] The polyethylene resin composition may include 0.01 to 0.5 parts by weight of the slip agent relative to 100 parts by weight of the polyethylene resin composition. The slip agent may include erucamide, oleamide, behenamide, stearamide, or a combination thereof.

[0017] Another embodiment provides a method for preparing a polyethylene resin composition for bottle caps, wherein the method comprises the steps of preparing a polyethylene resin using a first reactor and a second reactor, wherein the polyethylene resin formed in the first reactor has a zero shear viscosity (η0 1st ) is 10 6 Moor ~ 10 7 Park, based on 13 The number of short chain branches per 1000 carbon atoms (SCB) of C-NMR 1st ) is 2.5 to 6.0, and the polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor have a zero shear viscosity ratio (η0 1st / η0 2nd ) is 11 to 20, the polymerization weight ratio of the polyethylene resin formed in the first reactor to the polyethylene resin formed in the second reactor is 40 to 60:40 to 60, and the strain hardening modulus is 20 MPa to 30 MPa.

[0018] Another implementation example provides a molded product prepared from the polyethylene resin composition for bottle caps.

[0019] The molded product may be a bottle cap.

[0020] Effects of the Invention

[0021] According to one implementation example, the polyethylene resin composition for bottle caps has excellent fluidity when processed into molded products, can improve productivity through high-speed processing, has high impact strength and strain hardening modulus, and can easily achieve lightweight and ultra-thinness, so it can be used in molded products such as bottle caps. DETAILED DESCRIPTION

[0022] The implementation example is described in detail below so that a person skilled in the art can easily implement it. However, the implementation example can be implemented in many different forms and is not limited to the implementation example described here.

[0023] According to an embodiment, the polyethylene resin composition for bottle caps comprises polyethylene resin. The polyethylene resin can be formed by polymerization using a secondary reactor consisting of a first reactor and a second reactor connected to each other. Specifically, the polyethylene resin is formed for the first time by polymerization in the first reactor, and the polyethylene resin obtained at this time is transferred to the second reactor, and can be polymerized again here to obtain the polyethylene resin for the second time.

[0024] The polyethylene resin polymerized in the first reactor may be a copolymer of ethylene and C3-C20 α-olefins, and the polyethylene resin polymerized in the second reactor may be an ethylene homopolymer.

[0025] The polyethylene resin formed in the first reactor has a zero shear viscosity (η) of 180°C based on an ARES rheometer. 01st ) can be 10 6 Moor ~ 10 7 For example, it can be 10 6 Moor ~ 5x10 6 When the polyethylene resin formed in the first reactor has a zero shear viscosity within the above range, the molded product has excellent long-term storage stability, high impact strength and strain hardening modulus, and is easy to achieve lightweight and ultra-thin.

[0026] The polyethylene resin formed in the first reactor is based on 13 The number of short chain branches (SCB) per 1000 carbon atoms in C-NMR 1st ) can be 2.5 to 6.0, for example, can be 3 to 6. When the polyethylene resin formed in the first reactor has the number of short chain branches within the above range, the impact strength and strain hardening modulus are high, lightweight and ultra-thin are easily achieved, the bending strength is also high, and a bottle cap with excellent sealing performance can be obtained.

[0027] When the polyethylene resin is formed in the first reactor, a comonomer may be supplied and polymerized together. The comonomer may be, but is not limited to, α-olefins of C3 to C20, for example, C4 to C8, C6 to C8. The comonomer may be supplied to the first reactor at a supply ratio of 50 to 80 g / kg relative to C2, for example, 55 to 65 g / kg. When the comonomer is supplied to the first reactor at a supply ratio within the above range, the molded product has excellent long-term storage stability, high impact strength and strain hardening modulus, and is easy to achieve lightweight and ultra-thin.

[0028] In addition, when the polyethylene resin is formed in the first reactor, H2 can be supplied and polymerized. The H2 can be supplied to the first reactor at a supply ratio of 30 to 80 mg / kg relative to C2, for example, 35 to 70 mg / kg. When H2 is supplied to the first reactor at a supply ratio within the above range, the molded product has excellent fluidity and can be processed at high speed.

[0029] The melt flow index (MI) (2.16 kg load, 190° C.) of the polyethylene resin formed in the first reactor may be 0.01 to 0.1, for example, 0.02 to 0.08. When the melt flow index of the polyethylene resin formed in the first reactor is within the above range, the molded product has excellent long-term storage stability, high impact strength and strain hardening modulus, and is easy to achieve lightweight and ultra-thin.

[0030] The density of the polyethylene resin formed in the first reactor may be 0.920 g / cm 3 ~0.940g / cm 3 , for example, can be 0.930 g / cm 3 ~0.940g / cm 3 When the density of the polyethylene resin formed in the first reactor is within the above range, the impact strength and strain hardening modulus are high, and lightweight and ultra-thinness can be easily achieved.

[0031] When the polyethylene resin is formed in the second reactor, H2 may be supplied and polymerized. The H2 may be supplied to the second reactor at a supply ratio of 1500 to 3000 mg / kg relative to C2, for example, 1600 to 2600 mg / kg. When H2 is supplied to the second reactor at a supply ratio within the above range, the molded product has excellent fluidity and can be processed at high speed.

[0032] The polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor have a zero shear viscosity ratio (η0 1st / η0 2nd ) can be 11 to 20, for example, can be 14 to 19. When the zero shear viscosity ratio of the polyethylene resin formed in the first reactor to the polyethylene resin formed in the second reactor is within the above range, when processed into a molded product, the fluidity is excellent, the impact strength and strain hardening modulus are high, and lightweight and ultra-thin are easily achieved.

[0033] The polymerization weight ratio of the polyethylene resin formed in the first reactor to the polyethylene resin formed in the second reactor may be 40 to 60:40 to 60. When the polymerization weight ratio of the polyethylene resin formed in the first reactor to the polyethylene resin formed in the second reactor is within the above range, the impact strength and strain hardening modulus are high, lightweight and ultra-thin are easily achieved, and the fluidity is excellent, and high-speed processing is possible.

[0034] According to an embodiment, the polyethylene resin composition for bottle caps may further include at least one selected from an antioxidant, a neutralizer and a slip agent in addition to the polyethylene resin.

[0035] The antioxidant may be one or more selected from 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,6-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamido]hexane, 1,6-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamido]propane, tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol-di-phosphite and bis(2,4-di-tert-butylphenyl)pentaerythritol-di-phosphite.

[0036] When the antioxidant is included in the polyethylene resin composition, the antioxidant may be included in an amount of 0.01 to 0.5 parts by weight, for example, 0.05 to 0.2 parts by weight, relative to 100 parts by weight of the polyethylene resin composition. When the antioxidant is within the above content range, the antioxidant does not change color during storage, does not change viscosity during processing, and can obtain excellent processability.

[0037] The neutralizing agent may include calcium stearate, zinc stearate, magnesium aluminum hydroxycarbonate, zinc oxide, magnesium hydroxystearate, or a combination thereof.

[0038] When the neutralizer is included in the polyethylene resin composition, the neutralizer may be included in an amount of 0.01 to 0.3 parts by weight, for example, 0.05 to 0.2 parts by weight, relative to 100 parts by weight of the polyethylene resin composition. When the neutralizer is within the above content range, there is no discoloration or viscosity change, excellent processability can be obtained, and physical properties such as strength can be maintained.

[0039] The slip agent may include erucamide, oleamide, behenamide, stearamide, or a combination thereof.

[0040] When the slip agent is included in the polyethylene resin composition, the slip agent may be included in an amount of 0.01 to 0.5 parts by weight, for example, 0.05 to 0.2 parts by weight, relative to 100 parts by weight of the polyethylene resin composition. When the slip agent is within the above content range, the opening torque is small, the bottle cap is easy to open, and the odor problem caused by the bottle cap can be prevented.

[0041] According to an embodiment, the melt flow index (MI) of the polyethylene resin composition for bottle caps can be 0.5 g / 10 min to 5.0 g / 10 min, for example, 0.8 g / 10 min to 2.0 g / 10 min at 190° C. and 2.16 kg load. When the melt flow index of the polyethylene resin composition is within the above range, the polyethylene resin composition has excellent fluidity when processed into a molded product and is easy to process at high speed.

[0042] The density of the polyethylene resin composition can be 0.950 g / cm 3 ~0.965g / cm 3 , for example, can be 0.950 g / cm 3 ~0.960g / cm 3 When the density of the polyethylene resin composition is within the above range, the impact strength and strain hardening modulus are high, and lightweight and ultra-thinness can be easily achieved.

[0043] The strain hardening modulus of the polyethylene resin composition may be 20 MPa to 30 MPa, for example, 20 MPa to 28 MPa. When the density of the polyethylene resin composition is within the above range, the impact strength and strain hardening modulus are high, and lightweight and ultra-thin are easily achieved.

[0044] The melt flow rate ratio (MFRR) of the polyethylene resin composition may be 80 to 180. The melt flow rate ratio (MFRR) may be a melt flow index (MFI) measured at a load of 21.6 kg and 190° C. 21.6 ) divided by the melt flow index (MI) measured at 2.16 kg load and 190 °C 2.16 When the melt flow rate ratio of the polyethylene resin composition is within the above range, when processed into a molded product, the product has excellent fluidity and high strain hardening modulus, and is easy to achieve lightweight and ultra-thin.

[0045] The following describes a method for preparing the aforementioned polyethylene resin composition for bottle caps according to another implementation example.

[0046] The method for preparing the polyethylene resin composition comprises the steps of preparing the polyethylene resin by using a first reactor and a second reactor.

[0047] Specifically, the polyethylene resin is first prepared by polymerization in a first reactor, and then the polyethylene resin is transferred to a second reactor and may be polymerized to prepare a final polyethylene resin for a second time.

[0048] The polymerization in the first reactor and the second reactor can be carried out under a Ziegler-Natta catalyst. As for the Ziegler-Natta catalyst, a catalyst known as a Ziegler-Natta catalyst uses a transition metal compound belonging to Group IV, Group V or Group VI of the periodic table as a main catalyst, wherein the most commonly used Ziegler-Natta catalyst is a halogenated complex composed of magnesium and titanium or magnesium and vanadium.

[0049] In addition, during the polymerization in the first reactor, a comonomer may be added. The comonomer may be a C3 to C20 α-olefin, for example, a C4 to C8, C6 to C8 α-olefin.

[0050] The polymerization in the first reactor can be carried out under the conditions of 40Mpa-50Mpa pressure, 70°C-100°C temperature and 40-70 minutes residence time, for example, it can be carried out under the conditions of 42Mpa-48Mpa pressure, 80°C-95°C temperature and 50-65 minutes residence time.

[0051] In addition, the polymerization in the second reactor can be carried out under the conditions of 40Mpa-50Mpa pressure, 80°C-110°C temperature and 20-50 minutes residence time, for example, it can be carried out under 42Mpa-48Mpa pressure, 90°C-100°C temperature and 25-40 minutes residence time.

[0052] The zero shear viscosity (η0) of the polyethylene resin formed in the first reactor is 1st ), number of short chain branches (SCB 1st ), the supply ratio of the comonomer to C2, the supply ratio of H2 to C2, the density, melt flow index, the polymerization weight ratio and other related descriptions are the same as the above contents, and the supply ratio of H2 to C2, the polymerization weight ratio and other related descriptions of the polyethylene resin formed in the second reactor are the same as the above contents. In addition, the zero shear viscosity ratio (η0) of the polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor is 1st / η0 2nd ) is also the same as above.

[0053] According to another implementation example, a molded product prepared from the aforementioned polyethylene resin composition for bottle caps is provided.

[0054] The molded product may be a lightweight and ultra-thin bottle cap.

[0055] The specific embodiments of the present invention are disclosed below. However, the embodiments described below are only used to specifically illustrate the present invention, and the present invention is not limited thereto. In addition, the contents not described here can be fully deduced technically by those skilled in the art, and therefore will not be described in detail.

[0056] (Preparation of polyethylene resin composition)

[0057] Example 1

[0058] By continuous slurry polymerization, two reactors with a reactor capacity of 90 liters in each step were connected in series, and a known Ziegler-Natta catalyst composed of magnesium and titanium was prepared as a main catalyst by a conventional method, and polymerization was carried out using 1-hexene as a comonomer.

[0059] In the first reactor, ethylene was supplied as a monomer and 1-hexene was supplied as a comonomer to polymerize a polyethylene resin of a copolymer, and in the second reactor, ethylene was supplied to polymerize a polyethylene resin of an ethylene homopolymer. The polymerization ratio in each reactor was 47:53 by weight.

[0060] At this time, the polymerization temperature of the first reactor was 87° C., and the polymerization temperature of the second reactor was 95° C. As comonomers, 1-hexene was supplied at a supply ratio of 60 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 39 mg / kg relative to ethylene (C2) to the first reactor. H2 was supplied at a supply ratio of 2000 mg / kg relative to ethylene (C2) to the second reactor. The polymerization conditions in the first reactor and the second reactor and the physical properties of the polyethylene resins formed are shown in Tables 1 and 2 below.

[0061] 100 parts by weight of the powdered polyethylene resin obtained above were mixed with 0.025 parts by weight of antioxidant Iragnox-1010, 0.05 parts by weight of Irgafos-168, and 0.1 parts by weight of neutralizer calcium stearate using a Hensel mixer, and then a polyethylene resin composition in pellet form was prepared using a twin-screw extruder. The physical properties of the polyethylene resin composition are shown in Tables 3 and 4 below.

[0062] Example 2

[0063] According to the components in Table 1 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0064] In the first reactor, H2 was supplied at a supply ratio of 35 mg / kg relative to ethylene (C2), and in the second reactor, H2 was supplied at a supply ratio of 1850 mg / kg relative to ethylene (C2). The polymerization amount ratio in each reactor was 48:52 by weight. Other than this, the preparation was carried out in the same manner as Example 1.

[0065] Example 3

[0066] According to the components in Table 1 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0067] In the first reactor, 1-hexene was supplied as a comonomer at a supply ratio of 56 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 52 mg / kg relative to ethylene (C2). In the second reactor, H2 was supplied at a supply ratio of 1600 mg / kg relative to ethylene (C2). The polymerization amount ratio in each reactor was 45:55 by weight. Except for this, the preparation was carried out in the same manner as Example 1.

[0068] Example 4

[0069] According to the components in Table 1 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0070] In the first reactor, 1-hexene was supplied as a comonomer at a supply ratio of 65 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 62 mg / kg relative to ethylene (C2). In the second reactor, H2 was supplied at a supply ratio of 2300 mg / kg relative to ethylene (C2). The ratio of the polymerization amount in each reactor was 50:50 by weight. Except for this, the preparation was carried out in the same manner as Example 1.

[0071] Comparative Example 1

[0072] According to the composition in Table 2 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0073] In the first reactor, 1-hexene was supplied as a comonomer at a supply ratio of 20 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 78 mg / kg relative to ethylene (C2). In the second reactor, H2 was supplied at a supply ratio of 2200 mg / kg relative to ethylene (C2). The polymerization amount ratio in each reactor was 49:51 by weight. Except for this, the preparation was carried out in the same manner as Example 1.

[0074] Comparative Example 2

[0075] According to the composition in Table 2 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0076] In the first reactor, 1-hexene was supplied as a comonomer at a supply ratio of 3 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 47 mg / kg relative to ethylene (C2). In the second reactor, H2 was supplied at a supply ratio of 200 mg / kg relative to ethylene (C2). The polymerization amount ratio in each reactor was 49:51 by weight. Except for this, the preparation was carried out in the same manner as Example 1.

[0077] Comparative Example 3

[0078] According to the composition in Table 2 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0079] In the first reactor, 1-hexene was supplied as a comonomer at a supply ratio of 68 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 10 mg / kg relative to ethylene (C2). In the second reactor, H2 was supplied at a supply ratio of 1500 mg / kg relative to ethylene (C2). The polymerization amount ratio in each reactor was 50:50 by weight. Except for this, the preparation was carried out in the same manner as Example 1.

[0080] Comparative Example 4

[0081] According to the composition in Table 2 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0082] In the first reactor, 1-hexene was supplied as a comonomer at a supply ratio of 24 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 4 mg / kg relative to ethylene (C2). In the second reactor, H2 was supplied at a supply ratio of 1300 mg / kg relative to ethylene (C2). The polymerization amount ratio in each reactor was 49:51 by weight. Except for this, the preparation was carried out in the same manner as Example 1.

[0083] Comparative Example 5

[0084] According to the composition in Table 2 below, a polyethylene resin composition was prepared in the same manner as in Example 1.

[0085] In the first reactor, 1-hexene was supplied as a comonomer at a supply ratio of 12 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 200 mg / kg relative to ethylene (C2). In the second reactor, 1-hexene was supplied as a comonomer at a supply ratio of 29 g / kg relative to ethylene (C2), and H2 was supplied at a supply ratio of 210 mg / kg relative to ethylene (C2). The polymerization amount ratio in each reactor was 50:50 by weight. Other than this, the preparation was carried out in the same manner as Example 1.

[0086]

Table 1

[0087]

[0088]

[0089]

Table 2

[0090]

[0091] Evaluation 1: Physical property measurement of polyethylene resin composition

[0092] The following physical properties were measured for the polyethylene resin compositions prepared in Examples 1 to 4 and Comparative Examples 1 to 5. The results are shown in Tables 3 and 4.

[0093] Melt flow index (MI)

[0094] According to ASTM D1238, the measurements were performed at 190°C with loads of 2.16 kg and 21.6 kg, respectively.

[0095] Melt flow rate ratio (MFRR)

[0096] MI 21.6 (21.6kg load, melt flow index at 190°C) / MI 2.16 (2.16kg load, melt flow index at 190°C)

[0097] density

[0098] The measurement was performed according to ASTM D1505.

[0099] Zero shear viscosity

[0100] The zero shear viscosity was calculated using the Carreau model after measuring the viscosity using an ARES (advanced rheometer expansion system) rheometer at a scanning frequency of 180° C., a strain of 5%, and a range of 0.01 to 400 rad / s.

[0101] Short chain branches per 1000 carbons (SCB)

[0102] The number of short chain branches per 1000 carbon atoms of polyethylene resins was calculated using quantitative nuclear magnetic resonance (NMR) spectroscopy. A Bruker 600 MHz NMR spectrometer was used and the 13C-NMR optimized 10mm multinuclear high-temperature cryoprobe. About 1.2g of sample was added to 2.8ml of 4:1 mixed solvent of 1,2-dichlorobenzene and benzene-d6, dissolved at 150℃ for later use, and measured under the experimental conditions of number of scans 5000, D1 12 seconds, pulse width 90°, measurement temperature 130℃, and proton-decoupling mode.

[0103] for 13 Quantitative calculation of C-NMR spectra, using the majority of methylene (-(CH2) n The mol% content of the polyethylene resin was calculated by integrating the characteristic signals (38.2ppm, 34.6ppm, 34.2ppm) of the specific comonomer and 1-hexene comonomer which are not affected by the sequence of other comonomers.

[0104] Thus, the number of short chain branches (SCB) per 1000 carbon atoms was calculated according to the following mathematical formulas 1 to 4.

[0105] [Mathematical formula 1]

[0106] Number of moles of hexene-1 (H') = (H1 + H2) / 2

[0107] (In the above mathematical formula 1,

[0108] H1 is A, A is the integral value of 38.1ppm,

[0109] H2 is (B+C) / 3, B is the integrated value of 34.6ppm, and C is the integrated value of 34.2ppm.)

[0110] [Mathematical formula 2]

[0111] The number of moles of ethylene (E') = [{(D+E)-E} / 2] + H'

[0112] (In the above mathematical formula 2,

[0113] D+E is the integrated value from 33.9ppm to 27.3ppm, and E is the integrated value at 27.3ppm.)

[0114] [Mathematical formula 3]

[0115] Mole % of hexene-1 = H' / (H'+E')×100

[0116] [Formula 4]

[0117] Number of short chain branches per 1000 carbons (SCB) = H' / (E'×2+H'×6)×1000

[0118] Strain hardening modulus

[0119] The measurements were performed using a 1.0 mm thick test piece in accordance with ISO 18488:2015.

[0120] Spiral flow length

[0121] The injection molding machine used was Toyo SI80III-F200, which was an Archimedean spiral type with a mold width of 10 mm, a thickness of 2 mm, and a maximum length of 2000 mm. The injection molding pressure was 1000 kgf / cm 2 The molding was carried out under the conditions of injection temperature of 235°C, injection speed of 30 mm / s, mold temperature of 50°C and cooling time of 10 seconds.

[0122] Izod impact strength

[0123] The test piece was injection molded according to ASTM-4 test piece specification, and after aging for 48 hours, it was measured at 23° C. according to ASTM D256 standard.

[0124] Bending strength

[0125] The test piece was injection molded according to ASTM-4 test piece specification, and after aging for 48 hours, it was measured at 23° C. according to ASTM D790 standard.

[0126]

Table 3

[0127] Example 1 Example 2 Example 3 Example 4 MI(2.16kg)(g / 10min) 1.0 0.8 1.3 1.6 <![CDATA[Density (g / cm 3 )]]> 0.955 0.954 0.956 0.952 <![CDATA[Zero shear viscosity ratio (η0 1st / η0 2nd )]]> 15.8 16.8 15.0 14.3 Strain hardening modulus (MPa) 25.6 27.0 21.3 20.1 Spiral flow length (cm) 59 52 57 62 <![CDATA[Impact strength (KJ / m 2 )]]> 21 27 17 15 <![CDATA[Flexural strength (kgf / cm 2 )]]> 8,700 8,500 9,000 8,200

[0128]

Table 4

[0129] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 MI(2.16kg)(g / 10min) 1.7 0.4 0.06 0.05 3.8 <![CDATA[Density (g / cm 3 )]]> 0.961 0.963 0.946 0.958 0.956 <![CDATA[Zero shear viscosity ratio (η0 1st / η0 2nd )]]> 10.8 9.7 6.3 22.0 1.1 Strain hardening modulus (MPa) 14.4 11.7 >50 >50 7.4 Spiral flow length (cm) 57 45 28 23 61 <![CDATA[Impact strength (KJ / m 2 )]]> 11.6 7.1 >50 >50 7.7 <![CDATA[Flexural strength (kgf / cm 2 )]]> 10,100 11,000 7,200 9,300 9,000

[0130] It can be confirmed from the above Tables 3 and 4 that the polyethylene resin composition according to Examples 1 to 4 of an implementation example has excellent fluidity when evaluated by spiral flow length, and has high strain hardening modulus and impact strength compared to Comparative Examples 1 to 5, and it can be seen that molded products such as bottle caps can be easily lightweight and ultra-thin.

[0131] On the contrary, it can be confirmed that the polyethylene resin compositions of Comparative Examples 1 and 5 have good fluidity when the spiral flow length is evaluated, but the strain hardening modulus and impact strength are low. It can be confirmed that the polyethylene resin composition of Comparative Example 2 has low fluidity when the spiral flow length is evaluated, and cannot be processed at high speed, and has low strain hardening modulus and impact strength. For the polyethylene resin compositions of Comparative Examples 3 and 4, although the strain hardening modulus and impact strength are high, the physical properties required for the lightweight and ultra-thinning of the bottle cap are good, but when the spiral flow length is evaluated, the fluidity is very low, and it cannot be processed at a commercial level. The bending strength of Comparative Example 3 is very low, and the sealing of the bottle cap is also problematic.

[0132] The preferred embodiments of the present invention are described above, but the present invention is not limited thereto. Various modifications can be made within the scope of the claims, the invention content and the drawings, which of course also belong to the scope of the present invention.

Claims

1. A polyethylene resin composition for bottle caps, wherein: comprising a polyethylene resin formed by a first reactor and a second reactor, The polyethylene resin formed in the first reactor has a zero shear viscosity of 10 based on an ARES rheometer at 180°C. 6 Moor ~ 10 7 Park, based on 13 The number of short chain branches per 1000 carbon atoms in C-NMR is 2.5 to 6.

0. When the polyethylene resin is formed in the first reactor, the comonomer is supplied at a supply ratio of 50 to 80 g / kg relative to ethylene, and hydrogen is supplied at a supply ratio of 30 to 80 mg / kg relative to ethylene; When the polyethylene resin is formed in the second reactor, hydrogen is supplied at a supply ratio of 1500 to 3000 mg / kg relative to ethylene; The polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor have a zero shear viscosity ratio of 11 to 20 based on an ARES rheometer at 180° C., and the polymerization weight ratio of the polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor is 40 to 60:40 to 60. The strain hardening modulus is 20MPa to 30MPa.

2. The polyethylene resin composition for bottle caps according to claim 1, wherein: The melt flow rate ratio of the polyethylene resin composition is 80-180.

3. The polyethylene resin composition for bottle caps according to claim 1, wherein: The density of the polyethylene resin composition is 0.950 g / cm 3 ~0.965g / cm 3 .

4. The polyethylene resin composition for bottle caps according to claim 1, wherein: The polyethylene resin composition further comprises at least one selected from an antioxidant, a neutralizer and a slip agent.

5. The polyethylene resin composition for bottle caps according to claim 4, wherein: The polyethylene resin composition comprises 0.01 to 0.5 parts by weight of the antioxidant relative to 100 parts by weight of the polyethylene resin composition. The antioxidant is one or more selected from 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,6-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamido]hexane, 1,6-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamido]propane, tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol-di-phosphite and bis(2,4-di-tert-butylphenyl)pentaerythritol-di-phosphite.

6. The polyethylene resin composition for bottle caps according to claim 4, wherein: The polyethylene resin composition comprises 0.01 to 0.3 parts by weight of the neutralizer relative to 100 parts by weight of the polyethylene resin composition. The neutralizing agent includes calcium stearate, zinc stearate, magnesium aluminum hydroxycarbonate, zinc oxide, magnesium hydroxystearate or a combination thereof.

7. The polyethylene resin composition for bottle caps according to claim 4, wherein: The polyethylene resin composition comprises 0.01 to 0.5 parts by weight of the slip agent relative to 100 parts by weight of the polyethylene resin composition. The slip agent includes erucamide, oleamide, behenamide, stearamide or a combination thereof.

8. A method for preparing a polyethylene resin composition for bottle caps, wherein: The method comprises the steps of preparing a polyethylene resin by using a first reactor and a second reactor, The polyethylene resin formed in the first reactor has a zero shear viscosity of 10 based on an ARES rheometer at 180°C. 6 Moor ~ 10 7 Park, based on 13 The number of short chain branches per 1000 carbon atoms in C-NMR is 2.5 to 6.

0. When the polyethylene resin is formed in the first reactor, the comonomer is supplied at a supply ratio of 50 to 80 g / kg relative to ethylene, and hydrogen is supplied at a supply ratio of 30 to 80 mg / kg relative to ethylene; When the polyethylene resin is formed in the second reactor, hydrogen is supplied at a supply ratio of 1500 to 3000 mg / kg relative to ethylene; The polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor have a zero shear viscosity ratio of 11 to 20 based on an ARES rheometer at 180° C., and the polymerization weight ratio of the polyethylene resin formed in the first reactor and the polyethylene resin formed in the second reactor is 40 to 60:40 to 60. The strain hardening modulus is 20MPa to 30MPa.

9. A molded article prepared from the polyethylene resin composition for bottle caps according to any one of claims 1 to 7.

10. The molded article according to claim 9, wherein The molded product is a bottle cap.

Citation Information

Patent Citations

  • Heat-resistant polyethylene resin composition and application thereof

    CN106317585A

  • Polyethylene resin composition and molded product produced from same

    CN106795298A

  • Polyethylene resin composition and bottle cap produced by the composition

    EP3988615A1

  • The polyethylene resin with excellent chemical resistance for medium blow molding

    KR101840126B1

  • A resin composition for manufacturing a porous separator

    KR101970492B1