Conductive compositions, conductive sheets, metal reinforcing plates, wiring boards with metal reinforcing plates, and electronic devices.
By adding resin particles and optimized resin and hardener to the conductive composition, the problems of resin flow and thickness changes in the connection between the metal plate and the wiring board are solved, and the conductive combination of high adhesion and stamping processability is achieved improves the quality and production efficiency of electronic equipment.
Patent Information
- Application Number
- CN202310307224.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-27
AI Technical Summary
In the connection between the metal plate and the wiring board, the existing conductive composition is prone to cracks and resin flow during stamping, resulting in a decrease in conductivity and thickness changes, which cannot be effectively suppressed and affects the quality and production efficiency of electronic equipment.
The conductive composition including a binder, metal particles and resin particles is adopted, wherein the regeneration rate of the resin particles is 5% or more and 95% or less. The bonding and stamping processability are improved by combining a preferred resin and a hardener. Resinhibits the flow of resin and keeps the thickness stable during heating and pressing.
The defect-free metal reinforced plate manufacturing is realized in stamping processing, which improves production efficiency and yield, prevents short circuits and malfunctions, and provides high-quality electronic equipment.
Smart Images

Figure CN116285233B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a conductive composition, a conductive sheet, a metal reinforcing plate, a wiring board with a metal reinforcing plate, and an electronic device. Background Art
[0002] The wiring board mounted inside the electronic device has flexibility, but from the perspective of connecting parts such as the connector, it is known to configure a reinforcing plate to suppress deformation. In the past, epoxy glass and the like were used as reinforcing plates, but from the perspective of imparting a function of suppressing electromagnetic wave noise, a metal plate is used. In the connection between the wiring board and the metal plate, a conductive composition having a resin as a main component is used as a bonding agent.
[0003] A filler may be added to the bonding agent for the purpose of achieving electrical conduction between the metal plate and the wiring board or for the purpose of controlling the elastic modulus.
[0004] For example, Patent Document 1 discloses that a conductor circuit and a reinforcing plate are connected via an adhesive layer, and describes that a conductive adhesive material containing conductive particles and an adhesive is used as the adhesive layer.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] [Patent Document 1] International Publication No. WO2021 / 167047 Summary of the invention
[0008] [Problems to be solved by the invention]
[0009] For the purpose of conducting between the metal plate and the wiring board, the bonding agent is required to have high conductivity. In recent years, from the perspective of application to vehicle parts or mobile phone parts, it is particularly required to continue to exhibit high conductivity even in harsh environments. Patent document 1 discloses a conductive composition, which can suppress the positional displacement of the conductive filler caused by temperature changes or vibrations by adding inorganic particles having fine pores, and exhibits high conductivity (connection stability).
[0010] The metal reinforcing plate formed by bonding a metal plate and a bonding agent (conductive composition) is mounted on wiring boards of various shapes, and is processed into a shape suitable for each wiring board. The processing mainly uses a method (punching processing) of punching the original plate of the metal reinforcing plate as a basis using a punch blade, but for example, when the conductive composition contains hard inorganic particles, there is a problem that the particles are not completely cut off and cracks are generated, and defects such as cracks are generated in the conductive composition starting from the cracks.
[0011] The metal reinforcing plate after stamping is joined to the wiring board in the heating and pressing process, but the following problem also arises: due to the pressure during heating and pressing, the resin of the conductive composition deforms and flows, protrudes from the metal plate, and contacts with undesired parts of the wiring board, causing a short circuit. (Resin flow)
[0012] In addition, since the conductive composition is crushed under the pressure during heating and pressing, the thickness of the composition is greatly reduced compared to before heating and pressing, and there is a problem that the total thickness of the completed wiring board with a metal reinforcement plate deviates greatly from the designed value, and a conductive composition with less thickness change before and after heating and pressing is required. (Film thickness guarantee)
[0013] The object of the present invention is to provide a conductive composition, a conductive sheet, a metal reinforcement plate, a wiring board with a metal reinforcement plate, and an electronic device that have excellent resin flow suppression, high adhesion and conductivity, and can achieve both excellent stamping processability and film thickness guarantee.
[0014] [Technical means to solve the problem]
[0015] The conductive composition of the present invention comprises a binder (A), metal particles (B), and resin particles (C), and the recovery rate of the resin particles (C) is 5% to 95%.
[0016] [Effects of the Invention]
[0017] According to the present invention, there can be provided a conductive composition and a conductive sheet which are excellent in suppressing resin flow, have high adhesiveness and conductivity, and can achieve both excellent punching workability and film thickness assurance.
[0018] The metal reinforcing plate formed by using the conductive composition and the conductive sheet can be processed without defects during stamping, thereby improving production efficiency. In addition, in the manufacture of a wiring board with a metal reinforcing plate including the metal reinforcing plate of the present invention, thickness changes during heating and pressing can be suppressed to achieve efficient production. Furthermore, high-quality electronic devices can be provided with good yields, in which resin flow is suppressed, short circuits caused by extension of components are prevented, and malfunctions can be prevented by high adhesion and conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram showing a cross section of a wiring board with a metal reinforcing plate according to the present invention.
[0020] [Explanation of Symbols]
[0021] 1: Conductive composition
[0022] 2: Metal Plate
[0023] 20: Patch Panel
[0024] 21: Insulation film
[0025] 22: Grounding circuit
[0026] 23: Overlay
[0027] 30: Opening
[0028] 100: Patch panel with metal reinforcement plate DETAILED DESCRIPTION
[0029] Hereinafter, the conductive composition, conductive sheet, metal reinforcing plate, wiring board with metal reinforcing plate, and electronic device of the present invention are described in sequence. In addition, unless otherwise specified, "-" indicating a numerical range includes its lower limit and upper limit. In addition, in order to make the description clear, the accompanying drawings are appropriately simplified. In addition, for the purpose of explanation, the scales of the various structures in the accompanying drawings may sometimes be greatly different.
[0030] [Conductive composition]
[0031] The conductive composition of the present invention comprises a binder (A), metal particles (B), and resin particles (C).
[0032] [Binder (A)]
[0033] The binder (A) serves as a matrix of the conductive composition and has the function of dispersing and supporting the metal particles (B) or the resin particles (C). The binder (A) is not particularly limited in composition as long as it has the above-mentioned function, but preferably contains the resin (a-1). The resin (a-1) in the present invention is usually solid, semi-solid or coagulated, and is defined as an organic material having a weight average molecular weight (Mw) of 5,000 or more in a softening or melting range.
[0034] [Resin (a-1)]
[0035] In addition to the weight average molecular weight (Mw), the composition and molecular structure of resin (a-1) are not particularly limited, and preferably a resin having one or more chemical bonds selected from the group consisting of an imide bond, an amide bond, a carbamate bond, and a urea bond. An imide bond, an amide bond, a carbamate bond, and a urea bond can interact with an adherend through the non-shared electron pair of the nitrogen atom contained in the bond to achieve a strong adhesive force. As a resin having the chemical bond group, for example, polyurethane resin, polyamide resin, polyimide resin, polyamide-imide resin, urea resin, polyurethane-urea resin, etc. can be cited.
[0036] In addition, the resin (a-1) is more preferably selected from two or more of the group consisting of an imide bond, an amide bond, a carbamate bond, and a urea bond. By having two or more of the adhesive (A) selected from the group consisting of an imide bond, an amide bond, a carbamate bond, and a urea bond, the interaction with the adherend is multiplexed, and a stronger adhesion can be exhibited. The so-called resin having two or more selected from the group consisting of an imide bond, an amide bond, a carbamate bond, and a urea bond, for example, refers to a polyamide-imide resin, a polyurethane urea resin, etc.
[0037] As described above, the resin (a-1) can be appropriately selected from the viewpoint of composition and molecular structure, but a suitable resin can also be selected according to the properties of the resin. From the viewpoint of applying thermal stimulation to the conductive composition to make it exhibit adhesiveness, the resin (a-1) is preferably a thermosetting resin (a-2) or a thermoplastic resin (a-3).
[0038] [Thermosetting resin (a-2)]
[0039] Thermosetting resin (a-2) is a thermosetting resin among resins (a-1). Thermosetting is defined as "a product that can be substantially converted into an infusible and insoluble product when cured by heating or other means such as radiation, catalysts, etc."
[0040] The thermosetting property can be exhibited by the reaction of the reactive functional groups with each other when the thermosetting resin (a-2) has reactive functional groups such as acidic groups. Alternatively, the thermosetting property can be exhibited by the reaction of the thermosetting resin (a-2) with the reactive functional groups incorporated into the curing agent (D) described later.
[0041] The acid value of the thermosetting resin (a-2) is preferably 5 mgKOH / g to 40 mgKOH / g. When the acid value is within the above range, the density of the cross-linked structure is within an appropriate range, and flexibility and toughness can be achieved. The acid value is more preferably 10 mgKOH / g to 20 mgKOH / g.
[0042] [Thermoplastic resin (a-3)]
[0043] Thermoplastic resin (a-3) is a thermoplastic resin among resins (a-1). Thermoplasticity is defined as "a state in which a plastic can be repeatedly softened by heating and hardened by cooling within a temperature range specific to plastics, and can be repeatedly molded, extruded or formed into an article in a uniform shape by flowing in a softened state".
[0044] The adhesive (A) preferably contains at least one functional group selected from the group consisting of an epoxy group, an oxetane group, an epithio group, and an aziridine group. In the case where the resin (a-1) has a reactive functional group such as an acidic group, the functional group causes a curing reaction in the reactive functional group or between the functional groups, and can exhibit high adhesion. As a method for making the adhesive (A) contain the functional group, for example, the following method can be adopted: adding the resin (a-1) having the functional group to the adhesive (A), or adding a curing agent having the functional group in the curing agent (D) described later to the adhesive (A).
[0045] [Hardener (D)]
[0046] The hardener (D) in the present invention is a substance that promotes or regulates the hardening reaction, and is defined as a substance having a molecular weight or a weight average molecular weight (Mw) of less than 5,000. The so-called hardening reaction is defined as "polymerization and / or crosslinking of a prepolymer or a polymer composition by heating or other means such as radiation, a catalyst, etc., so that the elastic modulus increases irreversibly". From the perspective of forming polymerization and / or crosslinking in the adhesive (A) by stimulation such as heat, so that the conductive composition exhibits strong adhesion, the adhesive (A) of the present invention preferably contains a hardener (D).
[0047] The curing reaction may be a reaction in which the curing agent (D) reacts with itself, or may react with other components in the binder (A) such as the resin (a-1). In the case where the resin (a-1) and the curing agent (D) undergo a curing reaction, the resin (a-1) is preferably a thermosetting resin (a-2) from the viewpoint of efficiently reacting.
[0048] From the viewpoint that the curing reaction does not proceed during storage but only occurs when heated, the combination of the thermosetting resin (a-2) and the curing agent (D) is preferably a combination that does not undergo a crosslinking reaction at 50°C but accelerates the curing reaction at 150°C.
[0049] Furthermore, by appropriately combining two or more curing agents having different curing reaction start temperatures, the crosslinking density of the conductive composition in each temperature range can be controlled.
[0050] Examples of the curing agent (D) include epoxy curing agents, oxetane curing agents, episulfide curing agents, aziridine curing agents, amine curing agents, isocyanate curing agents, and imidazole curing agents. Among them, epoxy curing agents, oxetane curing agents, episulfide curing agents, and aziridine curing agents are preferred because they can efficiently undergo a curing reaction with the thermosetting resin (a-2) and exhibit high adhesion.
[0051] As the epoxy curing agent, for example, a glycidyl ether epoxy compound, a glycidyl amine epoxy compound, a glycidyl ester epoxy compound, a cyclic aliphatic (alicyclic) epoxy compound, etc. are preferable.
[0052] Examples of the glycidyl ether epoxy compound include bisphenol A epoxy compounds, bisphenol F epoxy compounds, bisphenol S epoxy compounds, bisphenol AD epoxy compounds, cresol novolac epoxy compounds, phenol novolac epoxy compounds, α-1-naphthol novolac epoxy compounds, bisphenol A novolac epoxy compounds, dicyclopentadiene epoxy compounds, tetrabromobisphenol A epoxy compounds, brominated phenol novolac epoxy compounds, tris(glycidyloxyphenyl)methane, tetrakis(glycidyloxyphenyl)ethane, and the like.
[0053] Examples of the glycidylamine-type epoxy compound include tetraglycidyldiaminodiphenylmethane, triglycidylparaaminophenol, triglycidylmethylaminophenol, and tetraglycidylmeta-xylylenediamine.
[0054] As said glycidyl ester type epoxy compound, diglycidyl phthalate, diglycidyl hexahydrophthalate, diglycidyl tetrahydrophthalate etc. are mentioned, for example.
[0055] Examples of the cyclic aliphatic (alicyclic) epoxy compound include epoxycyclohexylmethyl-epoxycyclohexanecarboxylate and bis(epoxycyclohexyl)adipate.
[0056] Examples of the oxetane curing agent include 1,4-bis{[(3-ethyloxetan-3-yl)methoxy]methyl}benzene, 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, 4,4'-bis[(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl, an ester of (2-ethyl-2-oxetanyl)ethanol and terephthalic acid, an etherified product of (2-ethyl-2-oxetanyl)ethanol and a phenol novolac resin, and an esterified product of (2-ethyl-2-oxetanyl)ethanol and a polycarboxylic acid compound.
[0057] Examples of the episulfide curing agent include bis(1,2-epithioethyl)sulfide, bis(1,2-epithioethyl)disulfide, bis(2,3-epithiopropyl)sulfide, bis(2,3-epithiopropylthio)methane, bis(2,3-epithiopropyl)disulfide, bis(2,3-epithiopropyldisulfide)methane, bis(2,3-epithiopropyldisulfide)ethane, bis(6,7-epithio-3,4-dithiaheptyl)sulfide, bis( 6,7-epithio-3,4-dithiaheptyl) disulfide, 1,4-dithiane-2,5-bis(2,3-epithiopropyldithiomethyl), 1,3-bis(2,3-epithiopropyldithiomethyl)benzene, 1,6-bis(2,3-epithiopropyldithiomethyl)-2-(2,3-epithiopropyldithioethylthio)-4-thiahexane, 1,2,3-tris(2,3-epithiopropyldithio)propane, etc.
[0058] Examples of the aziridine curing agent include trimethylolpropane-tri-a-2-aziridinyl propionate, tetramethylolmethane-tri-a-2-aziridinyl propionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), and N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide).
[0059] Examples of the amine curing agent include diethylenetriamine, triethylenetetramine, methylenebis(2-chloroaniline), methylenebis(2-methyl-6-methylaniline), 1,5-naphthalene diisocyanate, and n-butylbenzyl phthalate.
[0060] Examples of the isocyanate curing agent include tolylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, dicyclohexylmethane diisocyanate, 1,5-naphthalene diisocyanate, tetramethylxylylene diisocyanate, and trimethylhexamethylene diisocyanate.
[0061] Examples of the imidazole curing agent include 2-methylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methylimidazole, and 1-cyanoethyl-2-undecylimidazolium trimellitate.
[0062] The curing agent (D) may be used alone or in combination of two or more. In order to adjust the storage elastic modulus or glass transition temperature of the conductive composition, the curing agent (D) preferably has a molecular weight or a weight average molecular weight of 100 or more.
[0063] The curing agent (D) is preferably formulated in an amount of 1 to 70 parts by mass, more preferably 3 to 50 parts by mass, relative to 100 parts by mass of the thermosetting resin (a-2). By setting the addition amount of the curing agent (D) to 1 part by mass or more, the density of the cross-linked structure of the conductive composition can be optimized, the adhesion can be improved, and the resin flow can be suppressed or the film thickness guarantee can be improved. By setting the addition amount of the curing agent (D) to 70 parts by mass or less, the conductive composition can be prevented from being excessively hardened, and the adhesion and stamping processability can be improved.
[0064] [Metal particles (B)]
[0065] The metal particles (B) are preferably conductive metals such as gold, platinum, silver, copper and nickel, and alloys thereof. In addition, for particles of a metal rather than a single composition that form a core, from the perspective of reducing costs, it is preferred that the coating layer covering the surface of the core be formed of a raw material having a higher conductivity than the core.
[0066] The core is preferably selected from nickel, silicon dioxide, copper and alloys thereof. Examples of the coating layer include gold, platinum, silver, tin, manganese, indium and alloys thereof. Among them, silver is preferably used from the viewpoint of conductivity and material cost.
[0067] The metal particles (B) may be used alone or in combination of two or more.
[0068] The composite particles preferably have a coating layer in a ratio of 1 to 40 parts by mass relative to 100 parts by mass of the core, more preferably 5 to 30 parts by mass. If coated with 1 to 40 parts by mass, the cost can be further reduced while maintaining electrical conductivity. In addition, the composite particles preferably have a coating layer that completely covers the core. However, in reality, sometimes a portion of the core is exposed. Even in this case, if the conductive material covers more than 70% of the surface area of the core, it is easy to maintain electrical conductivity.
[0069] The shape of the metal particles (B) is not limited as long as the desired conductivity can be obtained. Specifically, for example, spherical, flaky, leaf-shaped, dendritic, plate-shaped, needle-shaped, rod-shaped, grape-shaped, and amorphous blocks can be listed. In addition, from the viewpoint of improving conductivity, spherical, flaky, leaf-shaped, dendritic, and plate-shaped are more preferred.
[0070] The average particle size of the metal particles (B) is 50 The average particle size D is preferably 1 μm to 50 μm, more preferably 3 μm to 30 μm, and still more preferably 5 μm to 20 μm. 50 When the particle size is within the above range, a suitable conductive path can be formed, and the conductivity can be improved. 50It can be determined by using a laser diffraction-scattering particle size distribution measuring device.
[0071] The average particle size of the metal particles (B) is 90 The average particle size D is preferably 1 μm to 120 μm, and more preferably 5 μm to 70 μm. 90 Within the above range, the occurrence of blocking can be suppressed. For example, a conductive sheet having a conductive composition on a removable film is transported in a rolled state. Blocking refers to a phenomenon in which the conductive composition adheres to the back side of the removable film when the conductive sheet is unrolled from the roll.
[0072] When the conductive composition is in a layered form, the thickness of the conductive composition before heat pressing is divided by the average particle size D of the metal particles (B). 50 The value X obtained is preferably 1 to 35. When X is 35 or less, a conductive path of the metal particles (B) is effectively formed in the conductive composition, and the conductivity is improved. From the viewpoint of improving the conductivity, X is more preferably 18 or less. In addition, when X is 1 or more, the contact points between the adherend and the metal particles (B) are not excessively increased, and the contact area between the adherend and the adhesive (A) is increased, so the adhesion is improved. X is more preferably 5 or more.
[0073] The metal particles (B) are preferably contained in 40% to 90% by mass of the total solid content of the conductive composition. By setting the content to this, conductivity, adhesion, and punchability can be taken into account. The content of the metal particles (B) is more preferably 45% to 80% by mass, and more preferably 50% to 70% by mass.
[0074] [Resin particles (C)]
[0075] The resin particles (C) in the present invention are defined as a substance in which an organic resin is in the form of particles. The resin particles (C) are carried in a dispersed state in the binder (A) and are incompatible with the binder (A). The recovery rate of the resin particles (C) is greater than 5% and less than 95%. By setting the recovery rate within the above range, the conductive composition as a whole recovers its shape by utilizing the shape recovery effect of the resin particles (C) after deloading after heating and pressing, and the thickness reduction can be suppressed. Furthermore, by adding the resin particles (C), it is possible to suppress the excessive flow of the binder (A) when the conductive composition is heated and pressed, thereby suppressing the flow of the resin.
[0076] The resin flow suppression effect is an effect that can be exhibited even if the recovery rate of the resin particles (C) is less than 5%, but in particles with a recovery rate of less than 5%, the space generated by the compression of the resin particles (C) during heating and pressing is filled with the binder (A), and the thickness of the conductive composition is reduced. If the recovery rate of the resin particles (C) is 5% or more and 95% or less, the effect of suppressing the thickness reduction of the conductive composition (film thickness guarantee) can be achieved through the above-mentioned estimated effect. The recovery rate of the resin particles (C) is preferably 30% or more and 95% or less, and more preferably 40% or more and 95% or less. By having the recovery rate within the above range, the film thickness guarantee is further improved.
[0077] The recovery rate of the resin particles (C) can be determined by a load-removal test using a micro compression tester described later in the items of Examples.
[0078] The recovery rate of the resin particles (C) can be controlled by appropriately selecting the type of organic resin, the type of raw material (monomer) used, whether a cross-linked structure is formed in the particles, the addition of inorganic fine particles, and the like.
[0079] The method for producing the resin particles (C) may be, for example, (1) forming particles when synthesizing an organic resin from a monomer as a raw material, or (2) pulverizing a bulk organic resin. Among these, the method (1) forming particles when synthesizing an organic resin from a monomer as a raw material is preferred from the viewpoint of being able to precisely control the particle size distribution of the resin particles (C).
[0080] The organic resin constituting the resin particles (C) is not particularly limited as long as it can exhibit a desired restoration rate, and for example, acrylic resins, polyurethane resins, nylon resins, polyimide resins, and styrene resins are preferred in terms of ease of production.
[0081] Average particle size D of resin particles (C) 50 The average particle size D of the resin particles (C) is preferably 1 μm or more and 15 μm or less. 50 The average particle size D is preferably within the above range because the shape recovery effect after heating and pressing can be effectively reflected in the conductive composition, and the film thickness guarantee is improved. 50 The average particle size D of the resin particles (C) can be determined by using a laser diffraction-scattering particle size distribution analyzer in the same manner as for the metal particles (B). 50 The thickness is more preferably 1 μm or more and less than 4 μm, and still more preferably 2 μm or more and 3 μm or less.
[0082] When the conductive composition is in a layered form, the thickness of the conductive composition before heat pressing is divided by the average particle size D of the resin particles (C). 50The value Y obtained is preferably 70 or less. When Y is 70 or less, the existence ratio of the resin particles (C) in the thickness direction in the conductive composition increases, and the restoration effect of the resin particles (C) is more effectively exhibited, thereby improving the film thickness guarantee. From the viewpoint of improving the film thickness guarantee, Y is more preferably 60 or less, and further preferably 25 or less.
[0083] Resin particles (C) preferably contain 0.1% to 35% by mass relative to the total solid content of the conductive composition. By setting the content of resin particles (C) to 0.1% by mass or more, resin flow, stamping processability and film thickness guarantee become good, and by setting the content of resin particles (C) to 35% by mass or less, adhesion is improved. The content ratio of resin particles (C) is more preferably 1% to 30% by mass, and further preferably 2% to 15% by mass.
[0084] The resin particles (C) may contain inorganic particles or pigments such as titanium oxide or iron oxide for the purpose of adjusting hardness or coloring, or may have inorganic particles or pigments such as silicon dioxide attached to the surface for the purpose of suppressing aggregation or adhesion of the resin particles (C).
[0085] The conductive composition in the present embodiment may also contain a heat stabilizer, an inorganic filler, a pigment, a dye, a tackifier resin, a plasticizer, a silane coupling agent, an ultraviolet absorber, a defoamer, a leveling agent, and the like as other optional components.
[0086] Examples of the inorganic filler include silicon dioxide, aluminum oxide, aluminum hydroxide, magnesium hydroxide, barium sulfate, calcium carbonate, titanium oxide, zinc oxide, antimony trioxide, magnesium oxide, talc, montmorillonite, kaolin, bentonite, etc. When the conductive composition contains an inorganic filler, the storage elastic modulus before curing can be controlled to an optimal flow rate.
[0087] [Conductive sheet]
[0088] The conductive sheet of this embodiment is a conductive sheet having a conductive composition on a releasable film. The conductive composition included in the conductive sheet is a non-flowing solid substance at room temperature and is in a layered form with a constant thickness.
[0089] [Releasable film]
[0090] The releasable film may be used without limitation as long as one or both surfaces of the releasable film are subjected to release treatment.
[0091] Examples of the peelable film include plastic sheets such as polyethylene terephthalate, polyethylene naphthalate, polyvinyl fluoride, polyvinylidene fluoride, rigid polyvinyl chloride, polyvinylidene chloride, nylon, polyimide, polystyrene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polycarbonate, polyacrylonitrile, polybutene, soft polyvinyl chloride, polyethylene, polypropylene, polyurethane, ethylene-vinyl acetate copolymer, and polyvinyl acetate; paper such as cellophane, high-quality paper, kraft paper, and coated paper; various nonwoven fabrics; synthetic paper; metal foil; or composite films obtained by combining these.
[0092] The surface of the release film may be subjected to matte treatment as required. Examples of matte treatment methods include sand matte, etching matte, coating matte, chemical matte, kneading matte, and the like.
[0093] The release film can be obtained by coating a release agent on a substrate. As the release agent, hydrocarbon resins such as polyethylene and polypropylene, higher fatty acids and metal salts thereof, higher fatty acid soaps, waxes, animal and plant oils and fats, mica, talc, silicone surfactants, silicone oils, silicone resins, fluorine surfactants, fluorine resins, fluorine-containing silicone resins, melamine resins, acrylic resins, etc. can be used. The release agent can be applied by conventionally known methods, such as gravure coating, kiss coating, die coating, lip coating, notch wheel coating, blade coating, roller coating, blade coating, spray coating, rod coating, spin coating, dip coating, etc.
[0094] From the viewpoint of achieving both thin film properties and conductivity, the thickness of the conductive composition in the conductive sheet is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and still more preferably 30 μm to 70 μm.
[0095] [Method for producing conductive sheet]
[0096] The conductive sheet of the present invention can be obtained, for example, by applying a conductive composition on a peelable film, drying it, and then performing B-stage curing as needed. The dried sheet-like conductive composition is also referred to as a conductive resin layer. The coating method can be appropriately selected from known methods, taking into account the film thickness of the adhesive, etc. Specific examples of coating methods include: gravure coating, kiss coating, die coating, lip coating, notch wheel coating, scraper coating, roller coating, blade coating, spray coating, rod coating, spin coating, dip coating, etc.
[0097] B-stage curing is a method of partially causing a curing reaction by heating the conductive composition at a predetermined temperature and time. By performing B-stage curing, the strength of the conductive composition can be improved while maintaining its adhesive force.
[0098] [Metal reinforcement plate]
[0099] In the metal reinforcement plate of the present invention, a conductive composition is attached to the metal plate. The metal plate may be, for example, conductive metals such as gold, silver, copper, iron and stainless steel. Among them, stainless steel is preferred in terms of strength, cost and chemical stability as a metal plate. The thickness of the metal plate is generally about 0.04 mm to 1 mm. The metal plate preferably has a nickel layer formed on the entire surface of the metal plate. The nickel layer is preferably formed by electrolytic nickel plating. The thickness of the nickel layer is about 0.5 μm to 5 μm, more preferably 1 μm to 4 μm. In addition, the conductive composition included in the metal reinforcement plate is a non-flowing solid substance at room temperature and is in a layered form with a certain thickness.
[0100] [Distribution panel with metal reinforcement plate]
[0101] The wiring board 100 with a metal reinforcing plate of this embodiment (see Figure 1 ) A ground circuit 22 is arranged on an insulating film 21, a covering layer 23 covers the ground circuit 22, a wiring board 20 is arranged in which a part of the ground circuit 22 is exposed through an opening 30, and a metal reinforcement plate is arranged on the wiring board 20. The conductive composition 1 of the metal reinforcement plate is in a layered state, and the wiring board 20 is joined to the metal plate 2. In the printed wiring board of this embodiment, the ground circuit 22 and the metal plate 2 are electrically connected via the conductive composition 1 by filling a part of the conductive composition 1 into the opening 30. Signal wiring can also be provided on the wiring board 20.
[0102] The area of the opening 30 of the wiring board 20 can be set to 0.16 mm, for example. 2 Above and 0.81mm 2 By setting the area of the opening 30 to 0.16 mm 2 As described above, the filling property of the conductive composition into the opening 30 can be improved. In addition, by setting the area of the opening 30 to 0.81 mm 2 Next, the area occupied by the opening 30 in the wiring board 20 can be reduced. The area of the opening 30 is preferably 0.25 mm 2 Above and 0.64mm 2 Below, more preferably 0.36mm 2 Above and 0.49mm 2 When the area of the opening 30 is within the above range, the filling property of the conductive composition into the opening 30 can be improved, and the contact resistance between the conductive composition and the ground circuit 22 can be reduced.
[0103] The shape of the opening 30 in a plan view may be a rectangular shape or a circular shape. When the shape of the opening 30 is a rectangular shape, it becomes particularly difficult to fill the four corners of the rectangular opening with the conductive composition, and gaps are easily formed at the four corners. However, by using the conductive composition of the present embodiment in which the resin flow is controlled within an appropriate range, the conductive composition can be well filled into the opening even in a rectangular opening.
[0104] [Electronic equipment]
[0105] Such a wiring board with a metal reinforcement plate can be mounted on electronic devices such as mobile phones, smart phones, notebook personal computers (PCs), digital cameras, liquid crystal displays, etc. In addition, it can also be suitably mounted on transportation equipment such as automobiles, trains, ships, and airplanes.
[0106] [Example]
[0107] The present invention is described in more detail below by way of examples and comparative examples, but the present invention is not limited to the following examples. In addition, the acid value and weight average molecular weight (Mw) of the resin (a-1), and the D values of the metal particles (B), the resin particles (C), and the comparative example silica particles (Z) are shown in Table 1. 50 The average particle size was measured by the following method.
[0108] [Acid value of resin (a-1)]
[0109] According to the neutralization titration method of Japanese Industrial Standards (JIS) K 0070, the acid value (mgKOH / g) measured is converted into solid content and obtained. Accurately measure about 1g of the sample in a co-stoppered conical flask, add 100mL of a mixed solution of tetrahydrofuran / ethanol (volume ratio: tetrahydrofuran / ethanol = 2 / 1) to dissolve. Add phenolphthalein test solution as an indicator, titrate with 0.1N alcoholic potassium hydroxide solution, and set the end point when the indicator remains light red for 30 seconds. Calculate the acid value (unit: mgKOH / g) according to the following formula.
[0110] Acid value (mgKOH / g) = (5.611×a×F) / S
[0111] in,
[0112] S: Sample quantity (g)
[0113] a: Consumption of 0.1N alcoholic potassium hydroxide solution (mL)
[0114] F: Titer of 0.1N alcoholic potassium hydroxide solution
[0115] [Weight average molecular weight (Mw) of resin (a-1)]
[0116] The measurement of Mw is performed using a gel permeation chromatograph (GPC) "HPC-8020" (manufactured by Tosoh Corporation). GPC is a liquid chromatograph that separates and quantifies substances dissolved in a solvent (THF; tetrahydrofuran) based on differences in their molecular sizes. This measurement is performed by connecting two "LF-604" (manufactured by Showa Denko: GPC column for rapid analysis: 6mmID×150mm size) in series and using them as columns, and is performed at a flow rate of 0.6mL / min and a column temperature of 40°C. The determination of Mw is performed by polystyrene conversion.
[0117] [D of metal particles (B), resin particles (C), and silica particles for comparative example (Z) 50 Average particle size]
[0118] About D 50 The average particle size is measured using a laser diffraction-scattering particle size distribution measuring device LS13320 (manufactured by Beckman-Coulter). It is a value obtained by measuring the conductive filler using a cyclone-dried powder sample module, and is the particle size at which the cumulative value in the cumulative distribution of particle sizes is 50%. In addition, the refractive index is set to 1.6.
[0119] [Recovery rate of resin particles (C)]
[0120] The recovery rate of the resin particle (C) is determined by a load-removal test using a micro compression tester "MCT-211" manufactured by Shimadzu Corporation. First, the resin particle (C) is placed on a lower pressure plate (SKS plate), and an independent resin particle (C) is selected using an optical microscope (objective lens magnification 50 times) of the "MCTM-211". The diameter d of the selected resin particle (C) is measured using the particle size measurement cursor of the "MCTM-211". The selected resin particle (C) is determined based on the particle size of the measurement object.
[0121] Next, the test indenter was lowered to the top of the selected resin particle (C) at the following load speed, and the particle size A when the maximum test force of 20 mN was applied to the resin particle (C) and the particle size B when the load was removed to the minimum test force of 0.3 mN were measured. Based on the displacement amount (recovery amount) L obtained from the particle size A and the particle size B, and the diameter d measured by the particle size measurement vernier, the recovery rate was calculated by the following formula:
[0122] Restoration rate (%) = restoration amount L (μm) / diameter d (μm) × 100,
[0123] The restoration rate of each resin particle (C) was determined. The restoration rates of three resin particles (C) were measured, and the average value was taken as the restoration rate.
[0124] <Measurement conditions of recovery rate>
[0125] Test temperature: room temperature (20°C), relative humidity 65%
[0126] Upper pressure head: Flat head with a diameter of 50μm (material: diamond)
[0127] Lower pressure plate: SKS flat plate
[0128] Test type: load-unload test
[0129] Maximum test force: 20mN
[0130] Minimum test force: 0.3mN
[0131] Load speed: 4.5mN / sec
[0132] Load holding time: 3 seconds
[0133] Unloading holding time: 1min
[0134] <Raw materials>
[0135] [Resin (a-1)]
[0136] (a-1)-1: Polyester resin: acid value 36 mgKOH / g, Mw=27,000 (manufactured by TOYO CHEM)
[0137] (a-1)-2: Polyimide resin: acid value 18 mgKOH / g, Mw=55,000 (manufactured by TOYO CHEM)
[0138] (a-1)-3: Polyamide resin: acid value 22 mgKOH / g, Mw=49,000 (manufactured by TOYO CHEM)
[0139] (a-1)-4: Polyurethane resin: acid value 16 mgKOH / g, Mw = 98,000 (manufactured by TOYO CHEM)
[0140] (a-1)-5: Polyurethane urea resin: acid value 15 mgKOH / g, Mw=100,000 (manufactured by TOYOCHEM)
[0141] (a-1)-6: Polyacrylic acid resin: acid value 55 mgKOH / g, Mw=120,000 (manufactured by TOYO CHEM)
[0142] [Hardener (D)]
[0143] D1: Bisphenol A type epoxy compound (jER828, molecular weight = 370, manufactured by Mitsubishi Chemical)
[0144] D2: Isophthalic acid type oxetane compound (ETERNACOLL OXIPA, molecular weight = 362, manufactured by Ube Industries)
[0145] D3: Hydrogenated bisphenol A episulfide compound (TBIS-AHS, molecular weight = 384, manufactured by Taoka Chemical Industry)
[0146] D4: Multifunctional aziridine compound (Chemitite PZ-33, molecular weight = 425, manufactured by Japan Catalyst)
[0147] D5: Polycarbodiimide compound (Carbodilite V-05, molecular weight = 1200, manufactured by Nisshinbo Chemical)
[0148] [Metal particles (B)]
[0149] B1: Silver-coated copper powder: D 50 =5.7μm, dendritic (manufactured by Mitsui Mining and Smelting)
[0150] B2: Silver-coated copper powder: D 50 =31.2μm, dendritic (manufactured by Mitsui Mining and Smelting)
[0151] B3: Silver-coated copper powder: D 50 =10.8μm, spherical (manufactured by Showa Denko Materials)
[0152] B4: Silver-coated copper powder: D 50 =7.5μm, spherical (manufactured by Showa Denko Materials)
[0153] B5: Silver-coated copper powder: D 50 = 11.3μm, flake-shaped (manufactured by DOWA Holdings)
[0154] [Resin particles (C)]
[0155] C1: Polyurethane resin particles: D 50 =3μm, recovery rate 91% (manufactured by TOYO CHEM)
[0156] C2: Acrylic resin particles: D 50 =3μm, recovery rate 87% (manufactured by TOYO CHEM)
[0157] C3: Acrylic resin particles: D 50 =3μm, recovery rate 45% (manufactured by TOYO CHEM)
[0158] C4: Acrylic resin particles: D 50 =3μm, recovery rate 38% (manufactured by TOYO CHEM)
[0159] C5: Acrylic resin particles: D 50 =3μm, recovery rate 6% (manufactured by TOYO CHEM)
[0160] C6: Acrylic resin particles: D 50 =3μm, recovery rate 3% (manufactured by TOYO CHEM)
[0161] C7: Acrylic resin particles: D 50 =4μm, recovery rate 83% (manufactured by TOYO CHEM)
[0162] C8: Acrylic resin particles: D 50 =16μm, recovery rate 76% (manufactured by TOYO CHEM)
[0163] C9: Acrylic resin particles: D 50 =1.0μm, recovery rate 90% (manufactured by TOYO CHEM)
[0164] C10: Acrylic resin particles: D 50 =1.2μm, recovery rate 88% (manufactured by TOYO CHEM)
[0165] C11: Acrylic resin particles: D 50 =2.7μm, recovery rate 86% (manufactured by TOYO CHEM)
[0166] C12: Acrylic resin particles: D 50 =3.9μm, recovery rate 85% (manufactured by TOYO CHEM)
[0167] C13: Polyimide resin particles: D 50 =3μm, recovery rate 75% (manufactured by TOYO CHEM)
[0168] [Silica particles for comparative example (Z)]
[0169] Z1:D 50 =2.6μm (Admafine SO-6, manufactured by Admatechs)
[0170] <Production of Conductive Composition and Conductive Sheet>
[0171] [Example 1]
[0172] 100 parts by mass of ((a-1)-5) as the resin (a-1), 212 parts by mass of (B1) as the metal particles (B), and 10.5 parts by mass of (C1) as the resin particles (C) were placed in a container, and methyl ethyl ketone as a solvent was added and mixed so that the non-volatile component concentration became 40% by mass. Subsequently, 30 parts by mass of (D1) as the curing agent (D) was added, and the mixture was stirred for 10 minutes using a stirrer to prepare a conductive composition solution.
[0173] Next, the prepared conductive composition solution was applied onto one of the release-treated surfaces of a releasable film (substrate material: foamed polyethylene terephthalate, substrate thickness 50 μm, release agent: alkyd release agent) using a doctor blade so as to have a thickness of 60 μm after drying, and dried in an electric oven at 100° C. for 2 minutes to obtain a conductive sheet having a conductive composition formed on the releasable film.
[0174] [Example 2 to Example 55, Comparative Example 1, Comparative Example 3]
[0175] Conductive sheets of Examples 2 to 55 and Comparative Examples 1 and 3 were obtained in the same manner as in Example 1 except that the types and amounts of the components to be blended were as described in Tables 1 to 8.
[0176] [Comparative Example 2]
[0177] A conductive sheet of Comparative Example 2 was obtained in the same manner as in Example 1, except that the resin particles (C) among the components to be formulated were changed to the silica particles (Z1) and the types and blending amounts of the other components were as described in Table 8.
[0178] <Evaluation>
[0179] The obtained conductive compositions (conductive sheets) were evaluated for resin flow, adhesion, conductivity, punching processability, and film thickness assurance according to the following methods. The evaluation results are shown in Tables 1 to 8. In addition, the value of X is: the thickness of the conductive resin layer before heating and pressing / the average particle size of the metal particles (B) [D 50], and the value of Y: the thickness of the conductive resin layer before heating and pressing / the average particle size of the resin-containing particles (C) [D 50 ] are also shown in these tables.
[0180] [Resin flow]
[0181] The conductive sheet prepared in each example and comparative example was cut into a size of 40 mm in width and 100 mm in length, and the conductive sheet was overlapped on a metal plate of 50 mm in width and 120 mm in length (a metal plate having a nickel layer of 2 μm formed on the surface of a commercially available SUS304 plate of 0.2 mm in thickness) in such a manner that the surface with the conductive composition exposed was in contact with the metal plate. Then, the conductive sheet was laminated using a roll laminator at 130°C and 3 kgf / cm 2 The conductive sheet and the metal plate were roll laminated under conditions of 0.5 m / min and 0.5 m / min, and then the release film was peeled off from the conductive composition to obtain a metal plate with a conductive composition.
[0182] Next, the metal plate with the conductive composition (metal reinforcement plate) was cut into a size of 5 mm×12 mm using a punching machine, and the surface with the conductive composition exposed was thermally laminated on a polyimide film (Toray-Dupont, “Kapton 500H”) having a thickness of 125 μm at 100° C. to obtain a laminate. Subsequently, a heat-resistant release film (Opulent CR1012MT4 150 μm, Mitsui Chemicals Tohcello) was placed on the upper and lower sides of the metal plate of the laminate, and the films were thermally pressed under the conditions of 170° C., 2.0 MPa, and 5 minutes to obtain an evaluation sample (a laminate of “polyimide film / conductive composition / metal plate”).
[0183] Next, the evaluation sample was observed using a magnifying glass with a magnification of 200 to 1000 times, and the flow amount of the conductive composition extending from the end of the metal plate (the maximum movement distance of the edge of the conductive composition, the maximum length between the end of the metal plate and the end of the conductive composition extending) was measured. The appearance was evaluated according to the following evaluation criteria using the measured values as indicators.
[0184] ◎: Very good (flow rate is 100 μm or less)
[0185] ○: Excellent (flow amount is more than 100 μm and 200 μm or less)
[0186] Δ: Practical (flow rate is more than 200 μm and less than 300 μm)
[0187] ×: Not practical (flow exceeds 300 μm)
[0188] [Adhesion]
[0189] The conductive sheet prepared in each example and comparative example was cut into a size of 25 mm in width and 100 mm in length, and the conductive sheet was overlapped on a metal plate of 30 mm in width and 150 mm in length (a metal plate having a nickel layer of 2 μm thick formed on the surface of a commercially available SUS304 plate of 0.2 mm thickness) in such a manner that the surface with the conductive composition exposed was in contact with the metal plate. Then, the conductive sheet was laminated using a roll laminator at 130°C and 3 kgf / cm 2 The conductive sheet and the metal plate were roll laminated under the conditions of 130°C, 3 kgf / cm2 and 0.5 m / min, and the release film was peeled off from the conductive composition. A copper foil (thickness 25 μm) was overlapped on the exposed surface of the conductive composition. The roll laminator was used to roll the conductive sheet and the metal plate. 2 The conductive composition and the copper foil were roll laminated under conditions of 0.5 m / min and 0.5 m / min to obtain a sample for evaluation.
[0190] Next, the adhesiveness was evaluated according to the following evaluation criteria using a tensile tester (small table tester EZ-TEST, manufactured by Shimadzu Corporation) at a tensile speed of 50 mm / min and the adhesive strength of the conductive composition to the metal plate of the evaluation sample in a 90° peel test as an index.
[0191] ◎: Very good (adhesive strength is 3N / cm or more)
[0192] ○: Excellent (adhesive strength is 2 N / cm or more and less than 3 N / cm)
[0193] Δ: Practical (adhesive strength is 1 N / cm or more and less than 2 N / cm)
[0194] ×: Not practical (adhesion strength is less than 1N / cm)
[0195] [Conductivity]
[0196] The conductive sheet (20 mm in width and 20 mm in length) prepared in each example and comparative example was overlapped on a metal plate (a metal plate having a 2 μm-thick nickel layer formed on the surface of a commercially available SUS304 plate having a thickness of 0.1 mm) in such a manner that the surface with the conductive composition exposed thereon was in contact with the metal plate. 2 The conductive sheet and the metal plate were roll laminated under the conditions of 200 rpm and 1 m / min to obtain a metal plate with a conductive sheet.
[0197] Next, the release film of the conductive sheet in the metal plate with the conductive sheet was peeled off and removed, and then the metal plate with the conductive composition (hereinafter referred to as the "metal plate with the conductive composition") was punched out using a punching machine into a square with a side of 10 mm to obtain a metal plate with the conductive composition (hereinafter referred to as the "metal plate with the conductive composition"). Then, using a separately prepared flexible printed wiring board, the surface of the metal plate with the conductive composition exposed (the surface of the conductive composition opposite to the metal plate) was overlapped on the wiring board, and a roll laminator was used at 130°C and 3kgf / cm 2 , 1m / min, the metal plate with the conductive composition is pasted to the wiring board. Then, they are hot-pressed at 170°C, 2MPa, and 5 minutes, and then heated at 160°C for 60 minutes using an electric furnace to obtain an evaluation sample. In addition, the wiring board has a copper foil circuit with a thickness of 32μm formed on both sides of a polyimide film with a thickness of 75μm, and a square with a side of 0.7mm and an opening area of 0.49mm is stacked on the copper foil circuit. 2 An insulating cover film (covering layer) with an adhesive and a thickness of 37.5 μm is provided to form a through hole (opening). In addition, an insulating cover film with an adhesive and a thickness of 37.5 μm without a through hole is laminated on another copper foil circuit (in order to prevent the flexible printed wiring board from warping, the copper foil circuit and the cover film are arranged symmetrically with respect to the polyimide film).
[0198] Next, the resistance (connection resistance) between the metal plate and the copper foil circuit of the evaluation sample was measured using a resistance meter and a BSP probe (Model: MCP-TP05P, manufactured by Mitsubishi Chemical Analytech), and the conductivity was evaluated according to the following evaluation criteria using the measured value as an indicator.
[0199] ◎: Good (connection resistance value is less than 20mΩ)
[0200] ○: Practical (connection resistance is 20 mΩ or more and less than 100 mΩ)
[0201] Δ: Practical (connection resistance value is 100mΩ or more and less than 500mΩ)
[0202] ×: Not practical (connection resistance value is 500mΩ or more)
[0203] [Pressing workability]
[0204] The conductive sheet prepared in each example and comparative example was overlapped on a metal plate (a metal plate having a nickel layer of 2 μm thick formed on the surface of a commercially available SUS304 plate of 0.1 mm thickness) in such a manner that the surface with the conductive composition exposed was in contact with the metal plate. Then, a roll laminator (small table laminator "SA-1010", manufactured by Detection Instrument Industry, the same below) was used to press the sheet at 130°C and 3 kgf / cm 2 The conductive sheet and the metal plate were roll laminated under the conditions of 200 rpm and 1 m / min to obtain a metal plate with a conductive sheet.
[0205] Next, using a press machine (model: hand press QCD type, manufactured by Kyoei Printing Engineering Co., Ltd., the same below), 50 pieces of the metal plate with the conductive sheet were demolded into a size of 5 mm×12 mm at a gap of 2.5 μm to obtain evaluation samples.
[0206] Next, using a magnifying glass with a magnification of 200 to 1000 times, the defective rate (mixing rate of defective products) of the evaluation sample is used as an indicator, and the stamping processability is evaluated according to the following evaluation criteria. In addition, the so-called defective product refers to a defective product that has at least one of partial non-detachment, peeling of the metal plate and the conductive composition, and deformation of the shape of the end of the conductive composition after stamping after processing into a demolding shape.
[0207] ◎: Very good (defective rate less than 10%)
[0208] ○: Excellent (defective rate is 10% or more and less than 15%)
[0209] Δ: Practical (defective rate is 15% or more and less than 25%)
[0210] ×: Not practical (defective rate is more than 25%)
[0211] [Film thickness guarantee]
[0212] The conductive sheet prepared in each example and comparative example was cut into a size of 40 mm in width and 100 mm in length, and the conductive sheet was overlapped on a metal plate of 50 mm in width and 120 mm in length (a metal plate having a nickel layer of 2 μm formed on the surface of a commercially available SUS304 plate of 0.2 mm in thickness) in such a manner that the surface with the conductive composition exposed was in contact with the metal plate. Then, the conductive sheet was laminated using a roll laminator at 130°C and 3 kgf / cm 2 The conductive sheet and the metal plate were roll laminated under conditions of 0.5 m / min and 0.5 m / min, and then the release film was peeled off from the conductive composition to obtain a metal plate (metal reinforcement plate) with a conductive composition.
[0213] Next, the metal plate with the conductive composition (metal reinforcement plate) was cut into a size of 5 mm×12 mm using a punching machine, and the surface with the conductive composition exposed was thermally laminated on a polyimide film (Toray-Dupont, “Kapton 500H”) having a thickness of 125 μm at 100° C. to obtain a laminate. Subsequently, a heat-resistant release film (Opulent CR1012MT4 150 μm, Mitsui Chemicals Tohcello) was placed on the upper and lower sides of the metal plate of the laminate, and the films were thermally pressed under the conditions of 170° C., 2.0 MPa, and 5 minutes to obtain an evaluation sample (a laminate of “polyimide film / conductive composition / metal plate”).
[0214] Next, the evaluation sample was cut near the center of the long side, and the vicinity of the cross section was cut using a cross section polisher. The processed cross section was observed using a scanning electron microscope (SEM) to measure the thickness (H1) of the conductive composition. The thickness of the conductive composition in the conductive sheet before being attached to the metal plate was defined as H2, and ΔH=H1 / H2 was calculated for each example and comparative example, and the evaluation was performed according to the following evaluation criteria.
[0215] ◎: Very excellent (ΔH is 0.6 or more)
[0216] ○: Excellent (ΔH is 0.5 or more and less than 0.6)
[0217] Δ: Practical (ΔH is 0.4 or more and less than 0.5)
[0218] ×: Not practical (ΔH less than 0.4)
[0219] [Table 1]
[0220]
[0221]
[0222]
[0223]
[0224]
[0225]
[0226]
[0227] [Table 8] Table 8
[0228]
Claims
1. A sheet-like conductive composition comprising: a binder (A), metal particles (B), and resin particles (C), The recovery rate of the resin particles (C) is 5% or more and 95% or less, The adhesive (A) comprises at least one selected from the group consisting of an imide bond, an amide bond, a urethane bond, and a urea bond, The metal particles (B) are contained in an amount of 40% to 80% by mass.
2. The sheet-like conductive composition according to claim 1, wherein The binder (A) includes at least one selected from the group consisting of an epoxy group, an oxetane group, an epithio group, and an aziridine group. 3 . The sheet-like conductive composition according to claim 1 , comprising 0.1% by mass to 35% by mass of the resin particles (C). 4 .
4. The sheet-like conductive composition according to claim 1 or 2, wherein The average particle size D of the resin particles (C) 50 1 μm~15 μm.
5. The sheet-like conductive composition according to claim 1 or 2, wherein The thickness is 5 μm~200 μm.
6. The sheet-like conductive composition according to claim 1 or 2, wherein The resin particles (C) have a recovery rate of 30% to 95%.
7. The sheet-like conductive composition according to claim 1 or 2, wherein: The average particle size D of the resin particles (C) 50 It is greater than or equal to 1 μm and less than 4 μm.
8. The sheet-like conductive composition according to claim 1 or 2, wherein The thickness of the sheet-like conductive composition divided by the average particle size D of the metal particles (B) 50 The obtained value X is 1 to 35.
9. The sheet-like conductive composition according to claim 1 or 2, wherein: The thickness of the sheet-like conductive composition divided by the average particle size D of the resin particles (C) 50 The obtained value Y is 70 or less.
10. The sheet-like conductive composition according to claim 1 or 2, wherein The binder (A) contains 1 to 70 parts by mass of a curing agent (D) based on 100 parts by mass of the thermosetting resin (a-2). 11 . A conductive sheet comprising the sheet-like conductive composition according to claim 1 , and a peelable film. 12 . A metal reinforcing plate comprising the sheet-like conductive composition according to claim 1 , and a metal plate.
13. A wiring board with a metal reinforcing plate, comprising the metal reinforcing plate according to claim 12.
14. An electronic device comprising the wiring board with a metal reinforcing plate according to claim 13.