A high-performance one-component polyurethane waterproof coating and preparation method thereof

By using organically modified layered silicates in polyurethane waterproof coatings to peel them into nanostructures, the problems of high cost and complex process of single-component polyurethane waterproof coatings in the prior art are solved, and high tensile strength and stability are achieved The combination of the building waterproofing project is suitable for heavy load areas.

CN116285641BActive Publication Date: 2024-11-15BEIJING ORIENTAL YUHONG WATERPROOF TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310180045.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-15
Publication Date
2024-11-15
Estimated Expiration
2043-02-15

AI Technical Summary

Technical Problem

The existing high-performance single-component polyurethane waterproof coatings are costly and complex in the process, and cannot meet the needs of high tensile strength during construction, especially in building waterproofing projects in heavy load areas.

Method used

The layered silicate with special organic modification is peeled off into a two-dimensional sheet nanostructure during coating synthesis. The hard segment structure is enhanced through its small size, large specific surface area and high surface energy interaction with the polyurethane molecular segments. cohesive force to improve the mechanical properties of the coating.

Benefits of technology

It realizes a cheap, simple process high-performance single-component polyurethane waterproof coating, which has good stability and high tensile strength, and is suitable for building waterproofing projects in heavy load areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116285641B_ABST
    Figure CN116285641B_ABST
Patent Text Reader

Abstract

The present invention provides a high-performance one-component polyurethane waterproof coating and a preparation method thereof, and relates to the technical field of coatings. The main method is to utilize a special organic modified layered silicate to be peeled off into a two-dimensional sheet-like nanostructure during the coating synthesis process, and utilize its small size, large specific surface area and high surface energy to improve the interaction with the polyurethane molecular chain segment, enhance the cohesion of the polyurethane hard segment structure, and thus improve the mechanical properties of the polyurethane waterproof coating. By adjusting the formula composition design and the synthesis process conditions, a one-component polyurethane waterproof coating with good storage stability and high mechanical properties can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a high-performance single-component polyurethane waterproof coating and a preparation method thereof. Background Art

[0002] Polyurethane waterproof coatings have been widely recognized in the field of building waterproofing due to their excellent mechanical properties, resistance to dilute acid and alkali corrosion, and strong adhesion to concrete. The typical mechanical performance index of mainstream products on the domestic market is a tensile strength of 2-3 MPa, which is used for ordinary waterproofing projects such as kitchens and bathrooms, basement ceilings, side walls and roofs. In heavy-loaded areas such as parking lots, stadium stands and bridges, waterproof coatings with higher mechanical properties are required. At present, the mainstream technical route to meet the requirements of high-performance polyurethane waterproof coatings is to make them into two-component products. When used, the A component containing NCO-terminated prepolymer is mixed with the B component containing a rigid chain extender (such as 3,3'-dichloro-4,4'-diaminodiphenylmethane, MOCA) to form a film. High-performance two-component polyurethane waterproof coatings contain a large amount of amine chain extenders, and the reaction speed after mixing is fast, so they are often limited by a short open time during construction.

[0003] Compared with two-component polyurethane waterproof coatings that need to be pre-mixed in a certain proportion, single-component polyurethane waterproof coatings do not need to be stirred before construction and can be used immediately after opening the bucket, which is more convenient for workers to construct and improves efficiency. Therefore, it is the largest selling variety of polyurethane waterproof coatings in China. Since it is impossible to improve the mechanical properties by adding a large amount of chain extenders such as MOCA and BDO like two-component coatings or elastomer products, high-performance one-component polyurethane waterproof coatings have certain technical barriers. At present, there is no one-component polyurethane waterproof coating with a tensile strength higher than 6MPa in the domestic market. According to the wide designability of polyurethane products, high-performance one-component polyurethane coating products can choose special polyethers such as polytetrahydrofuran diol or polyetheramine. For example, as shown in CN107474713A, CN104877542A, CN106497371A and CN107286834A, high-performance one-component polyurea waterproof coating products generally use polyetheramine and isocyanate to form a prepolymer, and use urea bonds with higher hydrogen bond density and strength to replace the urethane bonds in polyurethane, thereby improving the cohesive strength of the hard segment and greatly improving the mechanical properties of the coating. However, the use of special polyethers or isocyanates greatly increases the formulation cost of single-component coatings, and the difference in reactivity between the primary amino group of polyether amine and the hydroxyl group of polyether polyol is too large, and the synthesis reaction of the prepolymer is difficult to control.

[0004] In view of the high cost and complex process of the existing technology, it is very necessary to find a high-performance one-component polyurethane waterproof coating and preparation method that is cheap, simple in process and has high tensile strength. Summary of the invention

[0005] The present invention aims at the problems existing in the prior art and provides a high-performance one-component polyurethane waterproof coating and a preparation method thereof. The main method is to utilize a special organic modified layered silicate to be peeled off into a two-dimensional sheet-like nanostructure during the coating synthesis process, and utilize its small size, large specific surface area and high surface energy to improve the interaction with the polyurethane molecular chain segment, enhance the cohesion of the polyurethane hard segment structure, and thus improve the mechanical properties of the polyurethane waterproof coating. By adjusting the formula composition design and the synthesis process conditions, a one-component polyurethane waterproof coating with good storage stability and high mechanical properties can be obtained.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A one-component polyurethane waterproof coating comprising the following components:

[0008] Polyurethane;

[0009] Quaternary ammonium salts;

[0010] Layered silicates;

[0011] Additives;

[0012] After the polyurethane waterproof coating is treated with toluene, the powder precipitated at the bottom is thermally desorbed and subjected to gas chromatography-mass spectrometry to detect the characteristic fragment 58amu. Among them, 58amu comes from [C3H8N] + , which is one of the characteristic peaks of quaternary ammonium salts (see literature: Bowen, RD and Maccoll, A. (1985), Low-energy, low-temperature massspectra: 4—Saturated alkylamines. Org. Mass Spectrom., 20: 331-335. and literature: Hvistendahl, G. and Undheim, K. (1970), High resolution mass spectrometry oftrimethylamine. Org. Mass Spectrom., 3: 821-824.).

[0013] In some specific embodiments, the treatment with toluene is specifically a dilution treatment with toluene, and the method for obtaining the bottom precipitated powder is as follows:

[0014] (1) Mix 20g of polyurethane waterproof coating with 120g of toluene. Take out 10ml of the mixture and put it into a 15ml centrifuge tube. Use a centrifuge (centrifuge disk radius is about 16cm) to separate the powder at a speed of 500rpm for 2min. After the end, pour out the upper liquid;

[0015] (2) Add 10 ml of toluene to the centrifuge tube and mix thoroughly by ultrasonic dispersion for 5 minutes.

[0016] (3) Centrifuge at 500 rpm for 2 min and discard the supernatant.

[0017] (4) Repeat steps (2) and (3) twice.

[0018] (5) Add 10 ml of anhydrous ethanol to the centrifuge tube, disperse by ultrasonic for 5 minutes, and then let it stand for 30 minutes. Pour off the upper liquid, and place the powder at the bottom in a vacuum oven at 30°C for 15 minutes to obtain the sample to be tested by thermal desorption gas chromatography-mass spectrometry.

[0019] Furthermore, in the one-component polyurethane waterproof coating, the mass fraction of NCO groups is 1-4%, preferably 1.4-4%.

[0020] Furthermore, after the one-component polyurethane waterproof coating is treated with toluene, the powder precipitated at the bottom is subjected to thermogravimetric analysis, and the mass loss rate of the powder at 500° C. is 1%-60%; preferably, the mass loss rate is 2%-56%.

[0021] Furthermore, according to the test of GB / T 16777-2008 "Test Methods for Building Waterproof Coatings", the tensile strength of the one-component polyurethane waterproof coating is ≥5 MPa.

[0022] Furthermore, the one-component polyurethane waterproof coating is treated with toluene, and the powder precipitated at the bottom is dried and analyzed by Fourier transform infrared spectroscopy. -1 There are at least two absorption peaks in the range of 2820-2880cm -1 The antisymmetric stretching vibration peak of methylene is 2880-2940cm -1 It is the symmetrical stretching vibration peak of methylene. This indicates that the quaternary ammonium salt modifier containing aliphatic carbon chains is successfully inserted into the interlayer of lamellar silicate, and the silicate precipitates due to the large difference in polarity with toluene.

[0023] Further, the quaternary ammonium salt contains oxygen, and the total content of oxygen in the cation of the quaternary ammonium salt is 7-14%. It is worth noting that the quaternary ammonium salt is composed of cations containing elements such as nitrogen and oxygen and anions such as chlorine or bromine.

[0024] Further, the quaternary ammonium salt includes one or more of butyl bis(2-hydroxyethyl)octadecyl ammonium chloride, hexadecyl-bis(2-hydroxyethyl)-octylammonium chloride, (2-hydroxyethyl){4-[(2-hydroxyethyl)(methyl)(octadecyl)nitrogen cation radical]butyl}methyloctadecyl ammonium chloride, [bis(2-hydroxyethyl)]dioctadecyl ammonium chloride, ethyl bis(2-hydroxyethyl)tetradecyl ammonium chloride and methyl bis(2-hydroxyethyl)octylammonium chloride.

[0025] Furthermore, the polyurethane is obtained by reacting a terminal hydroxyl polymer and isocyanate.

[0026] Furthermore, the hydroxyl-terminated polymer includes poly(oxypropylene-oxyethylene) polyol and / or polyoxypropylene polyol having a hydroxyl value ranging from 20 to 120 mgKOH / g.

[0027] Further, the isocyanate includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and dicyclohexylmethane diisocyanate.

[0028] Furthermore, the layered silicate is composed of tetrahedral silicate sheets and octahedral hydroxide sheets in a ratio of 2:1, including one or more of montmorillonite, saponite and artificially synthesized hectorite, and has an ion exchange capacity of 50-125 mmol / 100g.

[0029] Furthermore, the auxiliary agent includes a catalyst, and the catalyst includes one or more of dibutyltin dilaurate, stannous octoate, dimethyltin diceneodecanoate and bismorpholinyl diethyl ether.

[0030] Furthermore, the auxiliary agent also includes: one or more of an inorganic filler, a plasticizer, a solvent, and a curing agent.

[0031] Furthermore, the inorganic filler includes one or more of talc, calcite, dolomite, kaolin and quartz powder; the plasticizer includes one or more of chlorinated paraffin, chlorinated palm oil, and diisononyl phthalate; the solvent includes one or more of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents or dibasic acid ester solvents with a closed cup flash point of 60-100°C; the latent curing agent includes oxazolidine and / or imine latent curing agents.

[0032] Furthermore, the present invention also provides a method for preparing the above-mentioned one-component polyurethane waterproof coating, comprising the following steps:

[0033] (1) Mixing layered silicate with water and stirring to obtain a silicate dispersion, mixing quaternary ammonium salt with ethanol and adding the mixture to the silicate dispersion, heating and stirring, filtering, washing, drying and grinding the precipitate to obtain an organically modified layered silicate; in the organically modified layered silicate, the cationic quaternary ammonium salt modifier is distributed between the negatively charged silicate layers, connected by electrostatic action and maintaining electrical neutrality.

[0034] (2) After mixing the additive, organic modified layered silicate and terminal hydroxyl polymer, stir, heat and dehydrate; then cool down, add isocyanate, continue to stir, heat, add additive, stir and degas, and obtain the polyurethane waterproof coating.

[0035] Furthermore, the organically modified layered silicate cannot be dispersed in toluene at a mass volume ratio of 0.1 g:5 ml.

[0036] In some specific embodiments, the preparation method of the polyurethane waterproof coating comprises the following steps:

[0037] (1) Mixing layered silicate with water and stirring to obtain a silicate dispersion, mixing quaternary ammonium salt with ethanol and adding the mixture to the silicate dispersion, heating to 20-75° C. and stirring for 1-3 hours, filtering, washing, drying and grinding the precipitate to obtain an organically modified layered silicate; in the organically modified layered silicate, the cationic quaternary ammonium salt modifier is distributed between the negatively charged silicate layers, connected by electrostatic action and maintaining electrical neutrality.

[0038] (2) After mixing the organically modified layered silicate and the terminal hydroxyl polymer in a reaction kettle, stir and evacuate at 110-120°C and a pressure of -0.092-0.098 MPa for 2-8 hours to make the moisture content less than 300 ppm; then cool down, add solvent and isocyanate, and continue to react at 50-85°C for 1-5 hours; continue to add catalyst and stir at 55-80°C for 15-30 minutes to obtain the polyurethane waterproof coating.

[0039] In some other specific embodiments, the preparation method of the polyurethane waterproof coating comprises the following steps:

[0040] (1) Mixing layered silicate with water and stirring to obtain a silicate dispersion, mixing quaternary ammonium salt with ethanol and adding the mixture to the silicate dispersion, heating to 20-75° C. and stirring for 1-3 hours, filtering, washing, drying and grinding the precipitate to obtain an organically modified layered silicate; in the organically modified layered silicate, the cationic quaternary ammonium salt modifier is distributed between the negatively charged silicate layers, connected by electrostatic action and maintaining electrical neutrality.

[0041] (2) After the inorganic filler, organic modified layered silicate, terminal hydroxyl polymer and plasticizer are mixed in a reaction kettle, the mixture is stirred and vacuumized at 110-120°C and a pressure of -0.092-0.098 MPa for 2-8 hours to reduce the moisture content to <300 ppm. The mixture is then cooled, and a solvent and isocyanate are added. The mixture is reacted at 50-85°C for 1-5 hours. The catalyst and latent curing agent are then added. The mixture is stirred at 55-80°C for 15-30 minutes and degassed to obtain a polyurethane waterproof coating.

[0042] The technical effects achieved by the present invention are:

[0043] The present invention adopts cheap poly (oxypropylene-oxyethylene) polyol and / or polyoxypropylene polyol and raw materials such as TDI and MDI, and modifies layered silicate with special quaternary ammonium salt, disperses and peels into two-dimensional sheet nanostructure in polyether polyol, and utilizes its small size, large specific surface area and high surface energy to improve the interaction with polyurethane molecular chain segment, enhance the cohesion of polyurethane hard segment structure, and thus improve the mechanical properties of polyurethane waterproof coating. By adjusting the formula composition design and synthesis process conditions, a single-component polyurethane waterproof coating with good storage stability and high mechanical properties can be obtained.

[0044] It is worth noting that before the present invention, there were some patent applications for enhancing the mechanical properties of polymer materials represented by layered silicates represented by montmorillonite. For example, CN1206299C discloses a nano-modified water-based waterproof coating, which uses nano-silicon dioxide, nano-zinc oxide, nano-titanium dioxide and sodium-montmorillonite to modify the polymer emulsion. The patent did not report the enhancement effect. There are also some patents, such as CN111560197A and CN108603050A, which use hydrophilic polymers to modify montmorillonite to make it more efficient in stripping in aqueous systems. More patents use positively charged hydrophobic polymers and Na + , Ca 2+The metal ions between the montmorillonite layers are exchanged to change the layered silicate from hydrophilic to lipophilic, and the polarity "like attracts like" principle is used to make it easier for hydrophobic polymers to enter the interlayers for exfoliation. This is also a common method for preparing organic modified montmorillonite nanocomposites. For example, patent CN114702805A uses uncapped polylactic acid, vinyl alcohol and ethylsulfonyl chloride to react and modify sodium montmorillonite, and prepares nanocomposites under the condition of melting polymer resin (200°C). More patents use long-chain alkyl ammonium salts to modify sodium montmorillonite, and also use the strong shear force of the screw extruder to intercalate the molten resin into the organic modified montmorillonite, promoting the exfoliation of the sheets into nanostructures. For example, CN100386384C utilizes hexadecyl trimethyl ammonium bromide to modify sodium montmorillonite, and successfully compounds with polymers and copolymers of polyamide 6, polyamide 66, polyamide 11, polyamide 12, polyamide 1010, polyurethane, polystyrene, nitrile rubber, styrene-butadiene rubber and silicone rubber to prepare nanocomposite materials. Patent CN1297470A discloses a method for modifying montmorillonite with a mixture of quaternary ammonium salt and cyclic amidine compound, and preparing thermoplastic and thermosetting nanocomposite materials such as polyurethane and epoxy resin. Unfortunately, the above method cannot be transplanted to organic solvent-based or solvent-free one-component polyurethane waterproof coating. The inventor found that, first, the classical alkane-substituted quaternary ammonium salt modifier, such as hexadecyl trimethyl ammonium bromide, differs greatly from the polarity of polyether polyol, and the affinity is not enough, and it is not possible to fully intercalate and peel off in the synthesis process of one-component polyurethane waterproof coating, and the improvement of the mechanical properties of the coating is small. Secondly, the production process of single-component polyurethane waterproof coatings cannot produce the high shear force and high temperature during screw extruder processing. Therefore, if you want to prepare nano-composite polyurethane coatings, the requirements for quaternary ammonium salt modifiers are higher than those for preparing sheets. Thirdly, conventional alkane or aromatic hydrocarbon substituted quaternary ammonium salts are catalysts for isocyanate self-polymerization (see literature: Gao Xiping, Cao Guangyu, Zhang Yuqing, Li Junxian, Research on the trimerization of isophorone diisocyanate, Polyurethane Industry, 21: 26-29.), which affects the storage stability of single-component polyurethane waterproof coatings. They can only be used for two-component coatings such as CN110452611A and CN1376748A.

[0045] In the present invention, the inventors found that the polarity of the layered silicate organic modifier has an important influence on the performance of the one-component polyurethane waterproof coating. When the organic modified layered silicate cannot be dispersed in toluene (mass volume ratio 0.1g:5ml), and the characteristic ion fragment 58 amu can be detected by gas chromatography-mass spectrometry (GC-MS) after thermal desorption, it has the effect of significantly enhancing the mechanical properties of the coating after curing in the one-component polyurethane waterproof coating. The organic modified layered silicate with this characteristic must have a certain amount of oxygen (or sulfur) atoms in its interlayer cations, so that the quaternary ammonium salt has appropriate polarity and is not affinity with non-polar alkanes or aromatics, so it cannot be dispersed in non-polar toluene; but it has a strong affinity for polyether polyols, phthalates and tetrahydrofuran, etc., and can be efficiently peeled into a nano-sheet structure during the synthesis process of non-aqueous one-component polyurethane waterproof coating, thereby improving the mechanical properties of the coating. In addition, due to the strong interaction between polyether polyols and organic modifiers, not only does it inhibit the self-polymerization catalysis of quaternary ammonium salt modifiers on isocyanates, ensuring the storage stability of single-component polyurethane waterproof coatings, but it also allows the polyurethane molecular chains to form various strong interactions with the silicate after stripping, including hydrogen bonds, ionic bonds and covalent bonds, further improving the mechanical properties of the coating. If the content of elements such as oxygen (or sulfur) in the modifier is too high, the organic modified layered silicate tends to be hydrophilic or ethanol, and the polarity gap with polyether polyols is large, and it is also impossible to most effectively strip into a nanostructure to improve the mechanical properties of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is the total ion flow diagram of the coating of Example 1 after being diluted with toluene and detected by gas chromatography-mass spectrometry;

[0047] Figure 2 The characteristic fragment ion peaks in the region of 36-44 min of the acquisition time detected by gas chromatography-mass spectrometry after the coating of Example 1 was diluted with toluene;

[0048] Figure 3 This is the total ion flow diagram of the coating of Example 2 after being diluted with toluene and detected by gas chromatography-mass spectrometry;

[0049] Figure 4 The characteristic fragment ion peaks in the 36-44 min acquisition time region of the coating of Example 2 after being diluted with toluene by gas chromatography-mass spectrometry;

[0050] Figure 5 This is the total ion flow diagram of the coating of Example 3 after being diluted with toluene and detected by gas chromatography-mass spectrometry;

[0051] Figure 6The characteristic fragment ion peaks in the 36-44 min acquisition time region detected by gas chromatography-mass spectrometry after the coating of Example 3 was diluted with toluene;

[0052] Figure 7 This is a thermogravimetric curve of the bottom powder obtained by diluting the coating of Example 4 with toluene;

[0053] Figure 8 The Fourier transform infrared spectra of the bottom powder obtained by diluting the coatings of Example 4 and Comparative Example 6 with toluene;

[0054] Fig. 9 This is the total ion flow diagram of the coating of comparative example 5 after being diluted with toluene and detected by gas chromatography-mass spectrometry;

[0055] Fig.10 This is the total ion flow diagram of the paint of comparative example 6 after being diluted with toluene and detected by gas chromatography-mass spectrometry. DETAILED DESCRIPTION

[0056] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0057] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are for describing specific embodiments rather than for limiting the scope of protection of the present invention.

[0058] When the embodiment gives a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs.

[0059] It is worth noting that the raw materials used in the present invention are all common commercially available products, so their sources are not specifically limited.

[0060] Example 1

[0061] A method for preparing a one-component polyurethane waterproof coating comprises the following steps:

[0062] 100 g of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100 g was added to 3000 g of deionized water and stirred at room temperature for three hours to disperse evenly; 60 g of butyl di(2-hydroxyethyl) octadecyl ammonium chloride was dissolved in 600 g of anhydrous ethanol, and then the ethanol solution was added dropwise to the silicate dispersion, and the addition was completed in about an hour. When the addition began, the temperature was raised to 60°C and stirred for three hours. The precipitated product was vacuum filtered, and the filter cake was rinsed with deionized water until the filtrate was detected with AgNO3 solution without precipitation. The washed filter cake was vacuum dried at 100-120°C, ground and sieved to obtain the organic modified montmorillonite. The organic modified montmorillonite could not be dispersed in toluene at a mass volume ratio of 0.1 g:5 ml, and precipitated at the bottom. The total content of oxygen and nitrogen in the modifier cation was 11.1%.

[0063] 8 grams of the above organic modified montmorillonite was added to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g and 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content was lower than 300 ppm, the temperature was lowered to 60°C, 10 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 were added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst was added, bubbles were removed by vacuum, and the material was discharged for use.

[0064] The coating was diluted with toluene, and the bottom powder obtained was thermally desorbed and detected by gas chromatography-mass spectrometry. The total ion flow diagram was as follows: Figure 1 As shown in the analysis, the acquisition time range of 36-44 min was found to have a characteristic fragment ion peak of 58 amu, such as Figure 2 shown.

[0065] The coating was diluted with toluene, and the obtained bottom powder was tested by thermogravimetric analysis. The mass loss rate of the powder at 500°C was 56%.

[0066] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0067] The NCO content of the coating is 3.64%.

[0068] Example 2

[0069] A method for preparing a one-component polyurethane waterproof coating comprises the following steps:

[0070] 100 g of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100 g was added to 3000 g of deionized water and stirred at room temperature for three hours to disperse evenly; 60 g of hexadecyl-bis(2-hydroxyethyl)-octylammonium chloride was dissolved in 600 g of anhydrous ethanol, and then the ethanol solution was added dropwise to the silicate dispersion, and the addition was completed in about an hour. When the addition began, the temperature was raised to 60°C and stirred for three hours. The precipitated product was vacuum filtered, and the filter cake was rinsed with deionized water until the filtrate was detected with AgNO3 solution without precipitation. The washed filter cake was vacuum dried at 100-120°C, ground and sieved to obtain the organic modified montmorillonite. The organic modified montmorillonite could not be dispersed in toluene at a mass volume ratio of 0.1 g:5 ml, and precipitated at the bottom. The total content of oxygen and nitrogen in the modifier cation was 10.4%.

[0071] 8 grams of the above organic modified montmorillonite was added to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g and 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content was lower than 300 ppm, the temperature was lowered to 60°C, 10 grams of Mobil Solvesso 150 solvent and 39 grams of MDI-50 were added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.002 grams of dibutyltin dilaurate catalyst was added, bubbles were removed by vacuum, and the material was discharged for use.

[0072] The coating was diluted with toluene, and the bottom powder obtained was thermally desorbed and detected by gas chromatography-mass spectrometry. The total ion flow diagram was as follows: Figure 3 As shown. When analyzing the acquisition time range of 36-44min, a characteristic fragment ion peak of 58 amu was found, such as Figure 4 shown.

[0073] The coating was diluted with toluene, and the obtained bottom powder was tested by thermogravimetric analysis. The mass loss rate of the powder at 500°C was 55.5%.

[0074] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0075] The NCO content of the coating is 3.37%.

[0076] Example 3

[0077] A method for preparing a one-component polyurethane waterproof coating comprises the following steps:

[0078] 100 grams of synthetic laponite (laponite) with an ion exchange capacity of about 75 mmol / 100g was added to 3000 grams of deionized water and stirred at room temperature for three hours to disperse evenly; 60 grams of butyl di(2-hydroxyethyl) octadecyl ammonium chloride was dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution was added dropwise to the silicate dispersion, and the addition was completed in about an hour. When the addition began, the temperature was raised to 60°C and stirred for three hours. The precipitated product was vacuum filtered, and the filter cake was rinsed with deionized water until the filtrate was detected with AgNO3 solution without precipitation. The washed filter cake was vacuum dried at 100-120°C, ground and sieved to obtain organic modified laponite. The organic modified laponite could not be dispersed in toluene at a mass volume ratio of 0.1g:5ml, and precipitated at the bottom. The total content of oxygen and nitrogen in the modifier cation was 11.1%.

[0079] 8 grams of the above organic modified hectorite is added to a mixed liquid consisting of 96 grams of polyoxypropylene diol with a hydroxyl value of 56 mgKOH / g and 32 grams of poly (oxyethylene-oxypropylene) triol with a hydroxyl value of 35 mgKOH / g, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 10 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst are added, bubbles are removed by vacuum, and the material is discharged for use.

[0080] The coating was diluted with toluene, and the bottom powder obtained was thermally desorbed and detected by gas chromatography-mass spectrometry. The total ion flow diagram was as follows: Figure 5 As shown. When analyzing the acquisition time range of 36-44min, a characteristic fragment ion peak of 58 amu was found, such as Figure 6 shown.

[0081] The coating was diluted with toluene, and the obtained bottom powder was tested by thermogravimetric analysis. The mass loss rate of the powder at 500°C was 53.5%.

[0082] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0083] The NCO content of the coating is 3.51%.

[0084] Example 4

[0085] A one-component polyurethane waterproof coating: on the basis of Example 1, common raw materials in the formula of one-component polyurethane waterproof coating are added, such as plasticizers, inorganic fillers and latent curing agents. Plasticizers are mainly used to reduce costs and adjust viscosity; inorganic fillers are used to increase tear strength and hardness while reducing costs; latent curing agents are mainly used to reduce bubbles generated during the curing process of the coating. Plasticizers can be selected from chlorinated paraffin and phthalate plasticizers; inorganic fillers are often selected from common inorganic minerals such as calcite, talcum powder, quartz powder and kaolin with a mesh size of 400-1500; latent curing agents can be commercially available products, and a common product is ALT-403 from Anxiang Elite Company. The addition of the above raw materials does not affect the essence of the present invention.

[0086] Specifically, the method comprises the following steps: adding 8 grams of the organic modified montmorillonite of Example 1, 88 grams of 800 mesh calcite and 12 grams of 1200 mesh talc to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 32 grams of 52# chlorinated paraffin, stirring and heating to 110°C and dehydrating for 1 hour under a vacuum degree of >-0.095 Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 35 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirring for 15 minutes, and then the temperature is raised to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for standby use.

[0087] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and then detected by gas chromatography-mass spectrometry, where a 58amu ion fragment peak was observed.

[0088] After the coating sample was diluted with toluene, the bottom powder obtained was tested by thermogravimetric analysis. The thermogravimetric curve is as follows: Figure 7 As shown, the mass loss rate of the powder at 500°C is 5%.

[0089] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. The curve is as follows Figure 8 As shown, at 2820-2940cm -1 There are two characteristic peaks in the range.

[0090] The NCO content of the coating is 1.88%.

[0091] Example 5

[0092] A one-component polyurethane waterproof coating: on the basis of Example 2, raw materials such as plasticizer, inorganic filler and latent curing agent are added. Specifically, the following steps are included: 8 grams of organic modified montmorillonite of Example 2, 88 grams of 800-mesh calcite and 12 grams of 1200-mesh talc are added to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 32 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 35 grams of Mobil Solvesso 150 solvent and 39 grams of MDI-50 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. Add 0.002 g of dibutyltin dilaurate catalyst and 8 g of ALT-403 latent curing agent, remove bubbles in vacuo, and discharge the material for later use.

[0093] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and then detected by gas chromatography-mass spectrometry, where a 58amu ion fragment peak was observed.

[0094] The coating was diluted with toluene, and the obtained bottom powder was tested by thermogravimetric analysis. The mass loss rate of the powder at 500°C was 4%.

[0095] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0096] The NCO content of the coating is 1.76%.

[0097] Example 6

[0098] A one-component polyurethane waterproof coating: on the basis of Example 3, raw materials such as plasticizer, inorganic filler and latent curing agent are added. Specifically, the following steps are included: 8 grams of organic modified hectorite of Example 3, 88 grams of 800-mesh calcite and 12 grams of 1200-mesh talc are added to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 32 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 35 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. Add 0.05 g of dibutyltin dilaurate catalyst and 8 g of ALT-403 latent curing agent, remove bubbles in vacuo, and discharge the material for later use.

[0099] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and then detected by gas chromatography-mass spectrometry, where a 58amu ion fragment peak was observed.

[0100] The coating was diluted with toluene, and the obtained bottom powder was tested by thermogravimetric analysis. The mass loss rate of the powder at 500°C was 4.5%.

[0101] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0102] The NCO content of the coating is 1.84%.

[0103] Example 7

[0104] A one-component polyurethane waterproof coating: based on Example 4, the content of organic modified montmorillonite is reduced, and the content of solvent, plasticizer and inorganic filler is increased. Specifically, 6 grams of organic modified montmorillonite of Example 4, 116 grams of 800 mesh calcite and 24 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 48 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 45 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. Add 0.05 g of dibutyltin dilaurate catalyst and 8 g of ALT-403 latent curing agent, remove bubbles in vacuo, and discharge the material for later use.

[0105] The coating was diluted with toluene, and the obtained bottom powder was tested by thermogravimetric analysis. The mass loss rate of the powder at 500°C was 2.5%.

[0106] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0107] The NCO content of the coating is 1.39%.

[0108] Example 8

[0109] A one-component polyurethane waterproof coating: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of [bis(2-hydroxyethyl)]di(octadecyl)ammonium chloride is dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution is dripped into a silicate dispersion, and the dripping is completed in about one hour. When the dripping begins, the temperature is raised to 60°C and stirred for three hours. The precipitated product is vacuum filtered, and the filter cake is washed with deionized water until the filtrate is detected by AgNO3 solution without precipitation. The washed filter cake is vacuum dried at 100-120°C, and ground and sieved to obtain an organic modified montmorillonite. The organic modified montmorillonite cannot be dispersed in toluene at a mass volume ratio of 0.1g:5ml, and precipitates at the bottom, and the total content of oxygen and nitrogen in the modifier cation is 7.5%.

[0110] 6 grams of the above organic modified montmorillonite, 116 grams of 800 mesh calcite and 24 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 48 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 45 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for use.

[0111] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and then detected by gas chromatography-mass spectrometry, where a 58amu ion fragment peak was observed.

[0112] After the coating sample was diluted with toluene, the bottom powder obtained was tested by thermogravimetric analysis, and the mass loss rate of the powder at 500°C was 2.5%.

[0113] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0114] The NCO content of the coating is 1.47%.

[0115] Example 9

[0116] A one-component polyurethane waterproof coating: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of ethyl bis (2-hydroxyethyl) tetradecyl ammonium chloride is dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution is dripped into a silicate dispersion, and the dripping is completed in about one hour. When the dripping begins, the temperature is raised to 60°C and stirred for three hours. The precipitated product is vacuum filtered, and the filter cake is washed with deionized water until the filtrate is detected by AgNO3 solution without precipitation. The washed filter cake is vacuum dried at 100-120°C, and ground and sieved to obtain an organic modified montmorillonite. The organic modified montmorillonite cannot be dispersed in toluene at a mass volume ratio of 0.1g:5ml, and precipitates at the bottom, and the total content of oxygen and nitrogen in the modifier cation is 13.9%.

[0117] 6 grams of the above organic modified montmorillonite, 116 grams of 800 mesh calcite and 24 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 48 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 45 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for use.

[0118] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and then detected by gas chromatography-mass spectrometry, where a 58amu ion fragment peak was observed.

[0119] After the coating sample was diluted with toluene, the bottom powder obtained was tested by thermogravimetric analysis, and the mass loss rate of the powder at 500°C was 2%.

[0120] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0121] The NCO content of the coating is 1.45%.

[0122] Example 10

[0123] A one-component polyurethane waterproof coating: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of methyl bis (2-hydroxyethyl) octyl ammonium chloride is dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution is dripped into a silicate dispersion, and the dripping is completed in about one hour. When the dripping begins, the temperature is raised to 60°C and stirred for three hours. The precipitated product is vacuum filtered, and the filter cake is washed with deionized water until the filtrate is detected by AgNO3 solution without precipitation. The washed filter cake is vacuum dried at 100-120°C, ground and sieved to obtain an organic modified montmorillonite. The organic modified montmorillonite cannot be dispersed in toluene at a mass volume ratio of 0.1g:5ml, and precipitates at the bottom, and the total content of oxygen and nitrogen in the modifier cation is 19.8%.

[0124] 6 grams of the above organic modified montmorillonite, 116 grams of 800 mesh calcite and 24 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 48 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 45 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for use.

[0125] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and then detected by gas chromatography-mass spectrometry, where a 58amu ion fragment peak was observed.

[0126] After the coating sample was diluted with toluene, the bottom powder obtained was tested by thermogravimetric analysis, and the mass loss rate of the powder at 500°C was 2%.

[0127] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There are two characteristic peaks in the range.

[0128] The NCO content of the coating is 1.39%.

[0129] Comparative Example 1

[0130] A coating: The difference from Example 1 is that the formula does not contain organic modified layered silicate. Specifically, the following steps are included: a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g and 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g is stirred and heated to 110°C and dehydrated for 1 hour under a vacuum degree of >-0.095Mpa. After the water content is lower than 300 ppm, the mixture is cooled to 60°C, 10 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst is added, bubbles are removed under vacuum, and the mixture is discharged for use.

[0131] This paint sample has no powder added and no precipitation is found at the bottom after dilution with toluene.

[0132] Comparative Example 2

[0133] A coating: The difference from Example 1 is that the structure of the organic modifier is different. Specifically, the following steps are included: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of hexadecyltrimethylammonium bromide is dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution is added dropwise to the silicate dispersion, and the addition is completed in about one hour. When the addition begins, the temperature is raised to 60°C and stirred for three hours. The precipitated product is vacuum filtered, and the filter cake is rinsed with deionized water until the filtrate is detected with AgNO3 solution without precipitation. The washed filter cake is vacuum dried at 100-120°C, and the organic modified montmorillonite is obtained by grinding and sieving. The organic modified montmorillonite can be dispersed in toluene at a mass volume ratio of 0.1g:5ml.

[0134] 8 grams of the above organic modified montmorillonite was added to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g and 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content was lower than 300 ppm, the temperature was lowered to 60°C, 10 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 were added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst was added, bubbles were removed by vacuum, and the material was discharged for use.

[0135] After the coating sample was diluted with toluene, no precipitated powder was observed.

[0136] Comparative Example 3

[0137] A coating: The difference from Example 1 is that the structure of the organic modifier is different. Specifically, the following steps are included: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of hexadecyl dodecyl dimethyl ammonium chloride is dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution is dripped into the silicate dispersion, and the dripping is completed in about one hour. When the dripping begins, the temperature is raised to 60°C and stirred for three hours. The precipitated product is vacuum filtered, and the filter cake is rinsed with deionized water until the filtrate is detected with AgNO3 solution without precipitation. The washed filter cake is vacuum dried at 100-120°C, and the organic modified montmorillonite is obtained by grinding and sieving. The organic modified montmorillonite can be dispersed in toluene at a mass volume ratio of 0.1g:5ml.

[0138] 8 grams of the above organic modified montmorillonite was added to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g and 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content was lower than 300 ppm, the temperature was lowered to 60°C, 10 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 were added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst was added, bubbles were removed by vacuum, and the material was discharged for use.

[0139] After the coating sample was diluted with toluene, no precipitated powder was observed.

[0140] Comparative Example 4

[0141] A coating: The difference from Example 1 is that the structure of the organic modifier is different. Specifically, the following steps are included: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of 2,6-diaminohexanoic acid monohydrochloride is added dropwise to the dispersion, and the addition is completed in about one hour. When the addition begins, the temperature is raised to 60°C and stirred for three hours. After cooling to room temperature, the modified montmorillonite dispersion is centrifuged at 10000rpm to obtain a precipitate, the supernatant is discarded, and the precipitate is rinsed with deionized water until the conductivity of the cleaning liquid is less than 25uS. The precipitate is vacuum dried at 100-120°C, and the organic modified montmorillonite is obtained by grinding and sieving. The total content of nitrogen and oxygen elements in the organic modifier is 32.9%, and the hydrophilicity of the organic modifier causes the organic modified montmorillonite to be dispersed in water. The organic modified montmorillonite cannot be dispersed in toluene at a mass volume ratio of 0.1g:5ml.

[0142] 8 grams of the above organic modified montmorillonite was added to a mixed liquid consisting of 96 grams of poly(ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g and 32 grams of poly(ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content was lower than 300 ppm, the temperature was lowered to 60°C, 10 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 were added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst was added, bubbles were removed by vacuum, and the material was discharged for use.

[0143] The coating sample was diluted with toluene, and the bottom powder obtained was thermally desorbed and detected by gas chromatography-mass spectrometry. No characteristic fragment peak 58amu could be detected.

[0144] Comparative Example 5

[0145] A coating: The difference from Example 4 is that the formula does not contain organic modified layered silicate. Specifically, the following steps are included: 88 grams of 800 mesh calcite and 12 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 32 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095 Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 35 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for use.

[0146] The coating was diluted with toluene, and the bottom powder obtained was thermally desorbed and detected by gas chromatography-mass spectrometry. No characteristic fragment peak 58amu could be detected. Fig. 9 The peak at about 10 minutes of collection time is a small amount of organic solvent remaining in the powder.

[0147] After the coating sample was diluted with toluene, the bottom powder obtained was tested by thermogravimetric analysis, and the mass loss rate of the powder at 500°C was less than 0.2%.

[0148] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There is no absorption peak in the range.

[0149] Comparative Example 6

[0150] A coating: The difference from Example 4 is that the structure of the organic modifier is different. Specifically, the following steps are included: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of hexadecyltrimethylammonium bromide is dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution is added dropwise to the silicate dispersion, and the addition is completed in about one hour. When the addition begins, the temperature is raised to 60°C and stirred for three hours. The precipitated product is vacuum filtered, and the filter cake is rinsed with deionized water until the filtrate is detected with AgNO3 solution without precipitation. The washed filter cake is vacuum dried at 100-120°C, and the organic modified montmorillonite is obtained by grinding and sieving. The organic modified montmorillonite can be dispersed in toluene at a mass volume ratio of 0.1g:5ml.

[0151] 8 grams of the above-mentioned organic modified montmorillonite, 88 grams of 800 mesh calcite and 12 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 32 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 35 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for use.

[0152] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and then detected by gas chromatography-mass spectrometry. No 58 amu ion fragment peak was observed. Fig.10 shown.

[0153] After the coating sample was diluted with toluene, the bottom powder obtained was tested by thermogravimetric analysis, and the mass loss rate of the powder at 500°C was less than 0.2%.

[0154] The coating was diluted with toluene, and the bottom powder obtained was analyzed by Fourier transform infrared spectroscopy. -1 There is no absorption peak in the range, such as Figure 8 shown.

[0155] Comparative Example 7

[0156] A coating: The difference from Example 4 is that the structure of the organic modifier is different. Specifically, the following steps are included: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of hexadecyl dodecyl dimethyl ammonium chloride is dissolved in 600 grams of anhydrous ethanol, and then the ethanol solution is added dropwise to the silicate dispersion, and the addition is completed in about one hour. When the addition begins, the temperature is raised to 60°C and stirred for three hours. The precipitated product is vacuum filtered, and the filter cake is rinsed with deionized water until the filtrate is detected with AgNO3 solution without precipitation. The washed filter cake is vacuum dried at 100-120°C, and the organic modified montmorillonite is obtained by grinding and sieving. The organic modified montmorillonite can be dispersed in toluene at a mass volume ratio of 0.1g:5ml.

[0157] 8 grams of the above-mentioned organic modified montmorillonite, 88 grams of 800 mesh calcite and 12 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 32 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 35 grams of Mobil Solvesso 150 solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for use.

[0158] After the coating sample was diluted with toluene, the precipitated powder was subjected to thermal desorption and gas chromatography-mass spectrometry was used to detect no visible 58 amu ion fragment peak; thermogravimetric analysis showed that the mass loss rate of the powder at 500°C was less than 0.2%; Fourier transform infrared spectroscopy analysis showed that the mass loss rate at 2820-2940cm -1 There is no absorption peak in the range.

[0159] Comparative Example 8

[0160] A coating: The difference from Example 4 is that the structure of the organic modifier is different. Specifically, the following steps are included: 100 grams of sodium montmorillonite with an ion exchange capacity of about 95 mmol / 100g is added to 3000 grams of deionized water, and stirred at room temperature for three hours to disperse evenly; 60 grams of 2,6-diaminohexanoic acid monohydrochloride is added dropwise to the silicate dispersion, and the addition is completed in about an hour. When the addition begins, the temperature is raised to 60°C and stirred for three hours. After cooling to room temperature, the modified montmorillonite dispersion is centrifuged at 10000rpm to obtain a precipitate, the supernatant is discarded, and the precipitate is rinsed with deionized water until the conductivity of the cleaning liquid is less than 25uS. The precipitate is vacuum dried at 100-120°C, and the organic modified montmorillonite is obtained by grinding and sieving. The organic modified montmorillonite cannot be dispersed in toluene at a mass volume ratio of 0.1g:5ml. The total content of nitrogen and oxygen in the organic modifier is 32.9%. The organic modifier is hydrophilic, so the organic modified montmorillonite can be dispersed in water.

[0161] 8 grams of the above-mentioned organic modified montmorillonite, 88 grams of 800 mesh calcite and 12 grams of 1200 mesh talc are added to a mixed liquid consisting of 96 grams of poly (ethylene oxide-propylene oxide) diol with a hydroxyl value of 56 mgKOH / g, 32 grams of poly (ethylene oxide-propylene oxide) triol with a hydroxyl value of 35 mgKOH / g and 32 grams of 52# chlorinated paraffin, stirred and heated to 110°C and dehydrated for 1 hour under vacuum degree>-0.095Mpa. After the water content is lower than 300 ppm, the temperature is lowered to 60°C, 35 grams of solvent and 25 grams of TDI-80 are added, stirred for 15 minutes, and then heated to 80°C for reaction for 3 hours. 0.05 grams of dibutyltin dilaurate catalyst and 8 grams of ALT-403 latent curing agent are added, bubbles are removed by vacuum, and the material is discharged for use.

[0162] The coating was diluted with toluene, and the bottom powder obtained was thermally desorbed and detected by gas chromatography-mass spectrometry. The characteristic fragment peak 58amu could not be detected. Thermogravimetric analysis showed that the mass loss rate of the powder at 500°C was 0.7%. Fourier transform infrared spectroscopy showed that the peak at 2820-2940cm -1 There is no absorption peak in the range.

[0163] The method for diluting the coating with toluene to obtain the bottom precipitated powder in the above examples is as follows:

[0164] (1) Mix 20g of polyurethane waterproof coating with 120g of toluene. Take out 10ml of the mixture and put it into a 15ml centrifuge tube. Use a centrifuge (centrifuge disk radius is about 16cm) to separate the powder at a speed of 500rpm for 2min. After the end, pour out the upper liquid;

[0165] (2) Add 10 ml of toluene to the centrifuge tube and mix thoroughly by ultrasonic dispersion for 5 minutes.

[0166] (3) Centrifuge at 500 rpm for 2 min and discard the supernatant.

[0167] (4) Repeat steps (2) and (3) twice.

[0168] (5) Add 10 ml of anhydrous ethanol to the centrifuge tube, disperse by ultrasonic for 5 minutes, and then let it stand for 30 minutes. Pour off the upper liquid, and place the powder at the bottom in a vacuum oven at 30°C for 15 minutes to obtain the sample to be tested by gas chromatography-mass spectrometry (GC-MS), thermogravimetric analysis (TGA) and Fourier transform infrared spectroscopy (FTIR) by thermal desorption method. The purpose of step (5) is to use the characteristics of anhydrous ethanol with lower toxicity and lower boiling point to obtain powder samples more quickly.

[0169] The gas chromatography-mass spectrometry test conditions are as follows:

[0170] Instruments: RFONTIER LAB EGA / PY-3030D, Agilent 8890 GC System and Agilent 5977B GC / MSD

[0171] Furnace temperature: 250℃.

[0172] Interface temperature: 250℃.

[0173] Sample loading: 2-3 mg.

[0174] Split ratio: 20:1.

[0175] Carrier gas: high purity helium.

[0176] Air flow rate: 1ml / min.

[0177] Chromatographic column: HP-5MS.

[0178] Inlet temperature: 300℃.

[0179] Transfer line temperature: 310°C.

[0180] Mass spectrometry detection conditions: ionization voltage 70 eV; scanning range (m / z) 30-550; ion source temperature 230 °C; MS quadrupole temperature 150 °C.

[0181] Column oven temperature program: initial temperature 50℃, hold for 3 min; increase to 150℃ at 25℃ / min, hold for 2 min; increase to 300℃ at 20℃ / min, hold for 3 min; decrease to 50℃ at 40℃ / min, hold for 3 min; increase to 180℃ at 40℃ / min, hold for 3 min; increase to 300℃ at 10℃ / min, hold for 3 min.

[0182] Thermogravimetric analysis test conditions are as follows:

[0183] Instrument: TA Instruments TGA 55.

[0184] Heating rate: 20℃ / min.

[0185] Carrier gas: high purity nitrogen.

[0186] Sample gas flow rate (Sample Purge): 25mL / min.

[0187] Balance gas flow rate (Balance Purge): 40mL / min.

[0188] By utilizing the characteristic that the organically modified layered silicate in the present invention cannot be dispersed in toluene, all fillers in the coating can be quickly obtained by diluting the coating with toluene (ordinary inorganic fillers cannot be dispersed in general organic solvents either), and the content of the organic modifier can be quantitatively analyzed by thermogravimetric analysis. The greater the mass loss rate at 500°C, the smaller the amount of inert fillers such as calcium carbonate talc added to the coating compared to the organically modified layered silicate, and the coating has high performance but also high cost. When the mass loss rate is >2%, there is a sufficient content of organically modified layered silicate in the coating to ensure that the tensile strength of the coating is >5MPa. Under 500°C, organic matter can be fully pyrolyzed, but inorganic fillers such as calcium carbonate, kaolin and talc remain thermally stable.

[0189] Test method: The tensile strength of the one-component polyurethane waterproof coating prepared in each example was tested according to the requirements of GB / T 16777-2008 "Test Methods for Building Waterproof Coatings". At the same time, the coatings prepared in each example and comparative example were stored at 50°C under sealed conditions for 4 weeks, and the viscosity growth ratio was recorded to examine the storage stability. The results are shown in Table 1.

[0190] Table 1 Summary of mechanical properties of examples and comparative examples

[0191]

[0192] Comparison of Example 1 and Comparative Example 1, as well as Example 4 and Comparative Example 5, proves that the layered silicate organic modification method of the present invention can greatly improve the tensile strength of the single-component polyurethane waterproof coating without affecting the storage stability. After being modified with a quaternary ammonium salt with a certain polarity, the layered silicate cannot be dispersed in toluene, has good affinity with polyether polyols, etc., can efficiently peel and disperse to improve the mechanical properties of the coating after curing, and inhibits the autocatalytic effect of the quaternary ammonium salt on isocyanate. According to the inventor's experience, the viscosity increase of the single-component polyurethane waterproof coating is not higher than 100% when stored at 50°C for 4 weeks, which can ensure that it can be stored at room temperature for at least 9 months. Comparative Examples 2, 3, 6 and 7 use long-chain aliphatic quaternary ammonium salts commonly found in other patents as modifiers. The modified layered silicate can be dispersed in non-polar toluene, and has insufficient affinity with polyether polyols, resulting in the organic modified montmorillonite not being efficiently peeled into nanosheets, and the enhancement effect is limited. At the same time, such quaternary ammonium salt modifiers catalyze the self-polymerization of isocyanate, resulting in the curing of the coating after long-term storage. Comparative Examples 4 and 8 use hydrophilic modified montmorillonite, which has a large polarity difference from the overall hydrophobic polyether polyols and plasticizers. They cannot be effectively stripped and dispersed in the solvent-based polyurethane waterproof coating and cannot achieve the best reinforcement effect.

[0193] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.

Claims

1. A one-component polyurethane waterproof coating, characterized in that: Contains the following ingredients: Polyurethane; Quaternary ammonium salts; Layered silicates; Additives; After the one-component polyurethane waterproof coating is treated with toluene, the powder precipitated at the bottom can be thermally desorbed and subjected to gas chromatography-mass spectrometry to detect the characteristic fragment 58amu; after the one-component polyurethane waterproof coating is treated with toluene, the powder precipitated at the bottom can be analyzed by Fourier transform infrared spectroscopy, and the characteristic fragment 58amu can be detected at 2820-2940cm -1 There are at least two absorption peaks in the range; After the one-component polyurethane waterproof coating is treated with toluene, the powder precipitated at the bottom is subjected to thermogravimetric analysis, and the mass loss rate of the powder at 500° C. is 2%-56%; According to GB / T 16777-2008 "Test Methods for Building Waterproof Coatings", the tensile strength of the one-component polyurethane waterproof coating is ≥5.7MPa; In the one-component polyurethane waterproof coating, the mass fraction of NCO groups is 1.4-4%; The quaternary ammonium salt contains oxygen, and the total content of oxygen and nitrogen in the cation of the quaternary ammonium salt is 7-14%; the quaternary ammonium salt modifier is successfully inserted into the interlayer of the lamellar silicate.

2. The one-component polyurethane waterproof coating according to claim 1, characterized in that: The quaternary ammonium salt includes one or more of butyl bis(2-hydroxyethyl)octadecyl ammonium chloride, hexadecyl-bis(2-hydroxyethyl)-octylammonium chloride, (2-hydroxyethyl){4-[(2-hydroxyethyl)(methyl)(octadecyl)nitrogen cation radical free radical]butyl}methyloctadecyl ammonium chloride, [bis(2-hydroxyethyl)]dioctadecyl ammonium chloride, ethyl bis(2-hydroxyethyl)tetradecyl ammonium chloride and methyl bis(2-hydroxyethyl)octylammonium chloride.

3. The one-component polyurethane waterproof coating according to claim 1, characterized in that: The polyurethane is obtained by reacting a terminal hydroxyl polymer and an isocyanate, wherein the terminal hydroxyl polymer includes poly(oxypropylene-oxyethylene) polyol and / or polyoxypropylene polyol with a hydroxyl value ranging from 20 to 120 mg KOH / g; the isocyanate includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and dicyclohexylmethane diisocyanate.

4. The one-component polyurethane waterproof coating according to claim 1, characterized in that: The layered silicate is composed of tetrahedral silicate sheets and octahedral hydroxide sheets in a ratio of 2:1, and includes one or more of montmorillonite, saponite and artificially synthesized hectorite, and has an ion exchange capacity of 50-125 mmol / 100g.

5. The one-component polyurethane waterproof coating according to claim 1, characterized in that: The auxiliary agent includes a catalyst, and the catalyst includes one or more of dibutyltin dilaurate, stannous octoate, dimethyltin dineodecanoate and bismorpholinyl diethyl ether.

6. The one-component polyurethane waterproof coating according to claim 5, characterized in that: The auxiliary agent also includes: one or more of an inorganic filler, a plasticizer, a solvent, and a latent curing agent.

7. The one-component polyurethane waterproof coating according to claim 6, characterized in that: The inorganic filler includes one or more of talc, calcite, dolomite, kaolin and quartz powder; the plasticizer includes one or more of chlorinated paraffin, chlorinated palm oil, and diisononyl phthalate; the solvent includes one or more of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents or dibasic acid ester solvents with a closed cup flash point of 60-100°C; the latent curing agent includes oxazolidine and / or imine latent curing agents.

8. The method for preparing the one-component polyurethane waterproof coating according to any one of claims 2 to 7, characterized in that: The following steps are involved: (1) mixing a layered silicate with water and stirring to obtain a silicate dispersion, mixing a quaternary ammonium salt with ethanol and adding the mixture to the silicate dispersion, heating and stirring, filtering, washing, drying and grinding the precipitate to obtain an organically modified layered silicate; (2) After the additive, organic modified layered silicate and terminal hydroxyl polymer are mixed, they are stirred, heated and dehydrated; then the temperature is lowered, solvent and isocyanate are added, stirring and heating are continued, additives are added, stirring and degassing are performed, and a single-component polyurethane waterproof coating is obtained.

Citation Information

Cited By

  • Low-VOC (volatile organic compound) high-performance single-component polyurethane waterproof coating and preparation method thereof

    CN119286382A

  • Low voc high performance one-component polyurethane waterproof coating and preparation method thereof