A fast-response heating-resistant carbon corrosion-resistant nickel-chromium-based alloy material and its preparation method and application

By adding solid solution elements to nickel-chromium alloy and preparing using specific processes, the problem of short service life of traditional electric heating wires in high carbon concentration environments is solved, and the electric heating wire that is resistant to carbon corrosion and responds to heating is achieved. It is suitable for many types of heating wires. industrial application.

CN116287870BActive Publication Date: 2024-11-22KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310304699.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-11-22
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Traditional nickel-chromium alloy electric heating wire has a short service life under high carbon concentration and high temperature environments, and is difficult to meet the needs of rapid response to heating and cooling, and cannot meet the demanding application requirements in industries and medical fields.

Method used

By adding solid solution elements such as iron, silicon carbide, cobalt, zirconium, manganese, tungsten, tantalum, niobium and yttrium to the nickel-chromium alloy, the resistance temperature coefficient and thermal conductivity are regulated to form an alloy material with strong carbon corrosion resistance, and The electric heating wire is prepared by vacuum smelting and extrusion drawing processes.

Benefits of technology

It realizes the stability and corrosion resistance of the electric heating wire in high temperature and high pressure environment, extends the service life, and improves the ability to respond quickly to heating and cooling, and is suitable for a variety of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116287870B_ABST
    Figure CN116287870B_ABST
Patent Text Reader

Abstract

The present invention discloses a fast-response heating and carbon-corrosion-resistant nickel-chromium alloy material, and a preparation method and application thereof. The nickel-chromium-based alloy material of the present invention improves key indicators such as carbon corrosion resistance, resistance temperature coefficient and thermal conductivity by adding a variety of solid solution elements into the alloy. Under high temperature, high pressure and highly corrosive environments, the nickel-chromium alloy heating wire prepared by using the nickel-chromium-based alloy material of the present invention has high stability. Compared with the existing copper heating wire and nickel-chromium alloy heating wire on the market, the nickel-chromium alloy heating wire provided by the present invention has stronger corrosion resistance, can work at higher temperatures and harsher environments, and has a wider range of applications. Compared with tungsten and molybdenum heating wires, the price is more affordable, and it can be used stably for a long time at high temperatures (800°C) and has a longer service life. Compared with chromium heating wires, it has better thermal conductivity and higher strength, so it can heat and cool more quickly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloys, and in particular relates to a fast-responding heating-resistant carbon corrosion-resistant nickel-chromium-based alloy material and a preparation method and application thereof. Background Art

[0002] Today, all walks of life in the world are increasingly demanding efficient, reliable and durable heating wires. Heating wires are widely used in industry, medical, manufacturing, food processing, automotive industry and other fields. However, the demand for heating wires in various fields is different. In the pharmaceutical industry, the heating wire is required to generate high precision heat for the preparation to ensure the quality and efficacy of the preparation; in the metallurgical and manufacturing industries, the heating wire is required to work in extremely high temperatures and corrosive environments, and have the ability to respond quickly to heating and quickly cool down; in the emerging electronic cigarette industry, the heating wire is required to heat to a certain temperature in an extreme time, quickly vaporize the smoke oil, and improve the user's use of the smoke. Therefore, in order to meet the needs of different industries for heating wires, heating wires made of different materials and processes are needed to achieve the best effect.

[0003] At present, small heating elements are mainly made of metal heating wires, porous metal ceramics and thermoelectric material films, which can accurately control the heating temperature with the support of integrated chips. However, in more demanding environments with high carbon concentrations, carbon accumulation often causes a huge change in resistance, thereby changing the temperature control accuracy and reducing the service life of the heating wire.

[0004] Nickel-chromium alloy is a common heating wire material, composed of nickel, chromium and other elements. Nickel-chromium alloy heating wire has many advantages, including high strength and excellent oxidation resistance. However, with the diversification and harshness of the use environment, the traditional nickel-chromium alloy heating wire can no longer cope with the use conditions in special environments (such as high carbon concentration environment, high water and oxygen environment). Therefore, it is necessary to develop a new nickel-chromium alloy heating wire with carbon corrosion resistance. Summary of the invention

[0005] In view of the above problems, an object of the present invention is to provide a carbon corrosion-resistant nickel-chromium-based alloy material that responds quickly to heating. A second object of the present invention is to provide a preparation method and application of the nickel-chromium-based alloy material.

[0006] The first object of the present invention is achieved in this way. A fast-responding heating carbon corrosion-resistant nickel-chromium-based alloy material is based on nickel-chromium alloy. The alloy material comprises 59% to 81% nickel (Ni) and 15% to 31% chromium (Cr) by mass percentage. The key indicators such as carbon corrosion resistance, resistance temperature coefficient, thermal conductivity, etc. are improved by adding one or more solid solution elements. The solid solution elements include, by mass percentage, 0.50% to 6.00% iron (Fe), 0.02% to 0.08% carbon (C), 0.02% to 0.08% silicon (Si), 0.80% to 1.60% cobalt (Co), 0.05% to 0.12% zirconium (Zr), 0.20% to 0.80% manganese (Mn), 0.50% to 0.80% tungsten (W), 0.03% to 0.20% tantalum (Ta), 0.10% to 0.50% niobium (Nb), and 1.00% to 2.10% yttrium (Y).

[0007] In the nickel-chromium alloy system, nickel and chromium form a limited solid solution. When the mass fraction of chromium is less than 20%, as the chromium content increases, the resistivity increases and the temperature coefficient of resistance decreases. When the mass fraction of chromium is greater than 20%, the temperature coefficient of resistance increases. Therefore, we control the temperature coefficient of resistance of the alloy heating wire by controlling the content of chromium in the alloy, and can adjust the change of the heating wire resistance according to different usage requirements.

[0008] Iron can improve the processing properties of nickel-chromium-based alloy materials. Iron can infinitely dissolve with nickel in nickel-chromium alloys to form a phase with excellent mechanical properties. It has the same crystal structure as austenite, which can effectively improve the strength and toughness of the material.

[0009] Silicon carbide nanoparticles can stably exist as a second phase in nickel-chromium alloys, forming a second phase reinforcement, which greatly improves the strength and hardness of nickel-chromium alloys. At the same time, the addition of silicon carbide increases the resistivity of the material, allowing the alloy heating wire to quickly respond to temperature rise after power is turned on. In addition, silicon, as a strong deoxidizer, can increase the hardness, yield point and tensile strength of the alloy. Increasing the resistance of the alloy meets the requirements of the heating wire to respond quickly to heating. As a ceramic material, silicon carbide has a low thermal conductivity. Adding too much will affect the heat dissipation efficiency of the heating wire and reduce the thermal conductivity of the heating wire. Therefore, the content of carbon and silicon must be strictly limited to less than 0.08%.

[0010] Cobalt can significantly improve the cutting performance of nickel-chromium alloy materials. Cobalt combines the grains of other elementary metal compounds in the alloy composition, making the alloy have higher toughness. Cobalt is often introduced as the main alloying element of high-temperature alloys, so the addition of cobalt improves the stability and oxidation resistance of nickel-chromium alloys at high temperatures. Cobalt also plays an important role in improving the corrosion resistance of nickel-chromium alloys.

[0011] Zirconium is a powerful deoxidizing and denitrifying element. It can effectively remove oxygen, nitrogen, sulfur and phosphorus from nickel-chromium alloys, refine the grains in the alloys, and improve the toughness of the alloys at low temperatures.

[0012] Manganese also has the effect of deoxidation and desulfurization, preventing hot brittleness. Manganese has a high electrical resistance, and proper addition can increase the resistance value of nickel-chromium alloy and speed up the heating response speed after power is turned on.

[0013] Tungsten has high hardness, high density, high wear resistance and refractory properties. The addition of appropriate content can improve the strength, wear resistance and operating temperature of nickel-chromium alloy.

[0014] Tantalum has extremely excellent corrosion resistance. The addition of tantalum can improve the ability of nickel-chromium alloy to resist carbon corrosion, ensure that the heating wire can be used for a long time, and increase the service life of the heating wire.

[0015] The addition of niobium can increase the strength of the alloy by 20%~25%, while improving the mechanical and welding properties of the alloy, and can improve the heat resistance and corrosion resistance of the nickel-chromium alloy and reduce brittleness.

[0016] The addition of yttrium can significantly enhance the oxidation resistance and ductility of nickel-chromium alloy, and is more conducive to the processing and forming of heating wire.

[0017] The second object of the present invention is achieved by the method for preparing the nickel-chromium-based alloy material according to the following steps:

[0018] 1) Select high-purity raw materials, dry and dehydrate the raw materials, and then design the alloy composition ratio according to the actual use needs and working conditions of the nickel-chromium alloy heating wire. After crushing the high-purity alloy raw materials, weigh and use them according to the designed ratio. Avoid the introduction of impurity elements in the whole process;

[0019] 2) Put the prepared alloy raw materials into a vacuum melting furnace, and carry out the melting process at 1200℃ to 1400℃ for 6~10h. The specific temperature depends on the composition of the nickel-chromium alloy. In order to prevent the alloy from oxidizing during the melting process, argon is selected as the protective gas. The content of oxides during the melting process should be controlled below 0.1%;

[0020] 3) Cut the smelted alloy material into nickel-chromium alloy blocks of appropriate size, heat it to 800°C in an induction furnace, and put it into an extrusion die for extrusion at an extrusion pressure of 50~75MPa and an extrusion speed of 20~30mm / min. The extruded alloy wire is then put into a drawing die for drawing at a drawing speed of 160~200mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 500~750°C and tempered for 2~12h. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0021] The application of the fast-response heating and carbon corrosion-resistant nickel-chromium alloy material is in the preparation of heating elements for electronic cigarettes that atomize tobacco oil and heat electronic cigarettes that heat solid tobacco particles, or in measuring high-temperature thermocouples or heating elements for electric heating type heaters.

[0022] The beneficial effects of the present invention are:

[0023] 1. The nickel-chromium-based alloy material of the present invention has a suitable resistivity, and when used in various heating elements, it can ensure the ability to quickly respond to heating.

[0024] 2. The nickel-chromium-based alloy material of the present invention has a high tensile strength. When used in various heating elements, it can extend the life of the heating wire itself, meet the needs of long-term use, and reduce the cost of use.

[0025] 3. The nickel-chromium-based alloy material of the present invention has a high thermal conductivity. When used in various heating elements, the heating wire can be cooled more quickly after each heating, thereby optimizing the user experience and increasing the service life of the heating wire.

[0026] 4. The nickel-chromium-based alloy material of the present invention has excellent carbonate corrosion resistance. When used in various heating elements, it can reduce the corrosion of carbides on the heating wire, increase the service life of the heating wire, and reduce the cost of use.

[0027] 5. The nickel-chromium-based alloy material of the present invention improves its key indicators such as carbon corrosion resistance, resistance temperature coefficient and thermal conductivity by adding a variety of solid solution elements to the alloy. The nickel-chromium alloy heating wire prepared by the nickel-chromium-based alloy material of the present invention has high stability under high temperature, high pressure and strong corrosive environment. Compared with the existing copper heating wire and nickel-chromium alloy heating wire on the market, the nickel-chromium alloy heating wire provided by the present invention has stronger corrosion resistance, can work at higher temperatures and harsher environments, and has a wider range of applications. Compared with tungsten and molybdenum heating wires, the price is more affordable, and it can be used stably for a long time at high temperatures (800°C) and has a longer service life. Compared with chromium heating wires, it has better thermal conductivity and higher strength, so it can heat and cool more quickly, and can be used to prepare heating elements for e-cigarettes that atomize cigarette oil and solid cigarette particles to heat e-cigarettes, or to measure high-temperature thermocouples or heating elements for electric heating type heaters. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The resistivity test results of Examples 1 to 8 and Comparative Examples 1 to 5 of the present invention are shown in FIG.

[0029] Figure 2 The tensile strength test results of the present invention 1 to 8 and comparative examples 1 to 5;

[0030] Figure 3 The average thermal conductivity test results of Examples 1 to 8 of the present invention and Comparative Examples 1 to 5;

[0031] Figure 4 These are the carbonate corrosion resistance test results of Examples 1 to 8 of the present invention and Comparative Examples 1 to 5. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation methods of the present invention are described in detail below in conjunction with embodiments.

[0033] The invention discloses a fast-response heating carbon corrosion-resistant nickel-chromium-based alloy material, which has the following chemical components in percentage by mass: 59% to 81% of nickel, 15% to 31% of chromium, 0.6% to 6% of iron, 0.8% to 1.6% of cobalt, 0.05% to 0.12% of zirconium, 0.2% to 0.8% of manganese, 0.5% to 0.8% of tungsten, 0.03% to 0.2% of tantalum, 0.1% to 0.5% of niobium, 1% to 2.1% of yttrium, and 0.02% to 0.08% of 20 to 100 nm silicon carbide nanoparticles. The nickel-chromium-based alloy material has excellent carbon corrosion resistance by adding a variety of solid solution elements, and can be quickly heated and cooled in a very short time.

[0034] The present invention also provides a method for preparing the carbon corrosion-resistant nickel-chromium-based alloy material with rapid response heating, which is achieved by the following steps:

[0035] (1) preparing the materials according to the chemical components, mixing the raw material powders and drying them in a drying oven at 60° C. to 80° C. for 15 to 25 hours to obtain a mixed material;

[0036] (2) The mixed material is placed in a vacuum induction furnace and smelted at 1200°C to 1400°C for 6 to 10 hours under argon protection to obtain the target carbon corrosion-resistant nickel-chromium-based alloy material.

[0037] The present invention further provides a nickel-chromium alloy heating wire based on the carbon corrosion-resistant nickel-chromium-based alloy material, and the preparation method thereof is as follows:

[0038] 1) Cut the nickel-chromium-based alloy material into appropriate lengths, heat it to 800°C, and place it in an extrusion die for extrusion at a pressure of 50-75 MPa and an extrusion speed of 20-30 mm / min. The extruded alloy wire is then placed in a drawing die of appropriate size for drawing at a speed of 160-200 mm / min to obtain a nickel-chromium alloy wire of a specified size;

[0039] 2) The nickel-chromium alloy wire is heated to 500-750° C. and tempered for 2-12 hours. After the tempering is completed, the wire is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0040] The present invention further provides the use of the fast-response heating carbon corrosion-resistant nickel-chromium alloy material in the preparation of heating elements for electronic cigarettes that atomize tobacco oil and heat electronic cigarettes that heat solid tobacco particles, or heating elements for measuring high-temperature thermocouples or electric heating heaters.

[0041] Example 1

[0042] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 60% Ni, 30% Cr, 0.04% C, 0.04% Si, 1.4% Co, 0.12% Zr, 0.2% Mn, 0.5% W, 0.12% Ta, 0.2% Nb, 1.8% Y, and the balance is Fe.

[0043] 1) Select raw materials according to the above alloy composition, with the purity of the raw materials ≥99.9% and the impurity element content ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 80°C for 15 hours;

[0044] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1200°C for 8 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0045] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 50MPa and an extrusion speed of 20mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 160mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 500°C and tempered for 2h. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0046] Example 2

[0047] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 65% Ni, 27% Cr, 0.06% C, 0.06% Si, 1.2% Co, 0.1% Zr, 0.4% Mn, 0.5% W, 0.12% Ta, 0.2% Nb, 1.8% Y, and the balance is Fe.

[0048] 1) Select raw materials according to the above alloy composition, with the purity of the raw materials ≥99.9% and the impurity element content ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 60°C for 25 hours;

[0049] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1300°C for 8 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0050] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 75MPa and an extrusion speed of 30mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 200mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 750°C and tempered for 12h. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0051] Example 3

[0052] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 70% Ni, 23% Cr, 0.08% C, 0.08% Si, 1% Co, 0.08% Zr, 0.6% Mn, 0.5% W, 0.12% Ta, 0.2% Nb, 1.8% Y, and the balance is Fe.

[0053] 1) Select metal raw materials according to the above alloy composition, with the purity of the raw materials ≥99.9% and the impurity element content ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 70°C for 20 hours;

[0054] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1300°C for 6 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0055] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to about 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 65MPa and an extrusion speed of 25mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 160mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 600°C and tempered for 7h. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0056] Example 4

[0057] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 75% Ni, 19% Cr, 0.06% C, 0.06% Si, 0.8% Co, 0.06% Zr, 0.6% Mn, 0.5% W, 0.12% Ta, 0.2% Nb, 1.8% Y, and the balance is Fe.

[0058] 1) Select metal raw materials according to the above alloy composition, with the purity of the raw materials ≥99.9% and the impurity element content ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 75°C for 15 hours;

[0059] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1250°C for 8 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0060] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 60MPa and an extrusion speed of 23mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 170mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 650°C and tempered for 8h. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0061] Example 5

[0062] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 80% Ni, 15% Cr, 0.04% C, 0.04% Si, 0.8% Co, 0.06% Zr, 0.6% Mn, 0.5% W, 0.12% Ta, 0.2% Nb, 1.8% Y, and the balance is Fe.

[0063] 1) Select metal raw materials according to the above alloy composition, with the purity of the raw materials ≥99.9% and the impurity element content ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 60°C for 25 hours;

[0064] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1200°C for 8 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0065] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to about 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 70MPa and an extrusion speed of 30mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 180mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 550°C and tempered for 10 hours. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0066] Example 6

[0067] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 60% Ni, 30% Cr, 0.04% C, 0.04% Si, 1.2% Co, 0.1% Zr, 0.2% Mn, 0.8% W, 0.2% Ta, 0.5% Nb, 2.1% Y, and the balance is Fe.

[0068] 1) Select metal raw materials according to the above alloy composition, with the purity of the raw materials ≥99.9% and the impurity element content ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 80°C for 18 hours;

[0069] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1340°C for 8 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0070] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to about 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 70MPa and an extrusion speed of 25mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 150mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 750°C and tempered for 2h. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0071] Example 7

[0072] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 70% Ni, 20% Cr, 0.06% C, 0.06% Si, 1.2% Co, 0.1% Zr, 0.8% Mn, 0.6% W, 0.18% Ta, 0.3% Nb, 1.5% Y, and the balance is Fe.

[0073] 1) Select metal raw materials according to the above alloy composition, the purity of the raw materials is ≥99.9%, and the content of impurity elements is ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 65°C for 20 hours;

[0074] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1300°C for 10 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0075] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to about 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 65MPa and an extrusion speed of 27mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 160mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 500°C and tempered for 10 hours. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0076] Example 8

[0077] A nickel-chromium-based alloy material with rapid response to heating, wherein the alloy elements include the following elements, measured by mass percentage: 80% Ni, 15% Cr, 0.08% C, 0.08% Si, 0.8% Co, 0.06% Zr, 0.6% Mn, 0.4% W, 0.16% Ta, 0.1% Nb, 1% Y, and the balance is Fe.

[0078] 1) Select metal raw materials according to the above alloy composition, with the purity of the raw materials ≥99.9% and the impurity element content ≤0.08%. Grind and mix the metal raw materials and SiC nanoparticles according to the ratio requirements, and dry them in a drying oven at 60°C for 22 hours;

[0079] 2) Place the dried alloy powder in a vacuum induction furnace for smelting at 1400°C for 6 hours. In order to prevent the alloy from oxidizing during the smelting process, argon is selected as the protective gas. The oxide content during the smelting process should be controlled below 0.1%;

[0080] 3) Cut the smelted alloy into nickel-chromium alloy blocks of appropriate size, heat them to about 800°C in an induction furnace, and put them into an extrusion die for extrusion at a pressure of 65MPa and an extrusion speed of 20mm / min. The extruded alloy wire is then put into a drawing die for drawing at a speed of 180mm / min to obtain a nickel-chromium alloy wire of the required size. The drawn alloy wire is heated to 600°C and tempered for 5h. After tempering, it is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

[0081] The following lists 5 groups of comparative examples for comparison with the nickel-chromium-based alloy materials of Examples 1 to 8 (the comparison of the element content of each group is shown in Table 1). Comparative Examples 1 to 5 are mainly based on Example 3 with typical component content and performance, and the material properties are changed by changing the content of one or more solid solution elements. The difference between Comparative Example 1 and Example 3 is that the content of the main alloying elements Ni and Cr is changed, the content of Ni is 55%, and the content of Co is 35%.

[0082] The difference between Comparative Example 2 and Example 3 is that the contents of several solid solution elements capable of regulating the resistivity of the nickel-chromium-based alloy material, including C, Si, and Mn, are reduced, wherein the content of C is 0.01%, the content of Si is 0.01%, and the content of Mn is 0.01%.

[0083] The difference between Comparative Example 3 and Example 3 is that the contents of several solid solution elements capable of regulating the resistivity of the nickel-chromium-based alloy material are increased, including C, Si, and Mn, wherein the content of C is 0.2%, the content of Si is 0.2%, and the content of Mn is 1.5%.

[0084] The difference between Comparative Example 4 and Example 3 is that the contents of several solid solution elements capable of regulating the thermal conductivity of the nickel-chromium-based alloy material are changed, including C and Si, wherein the content of C is 0.2% and the content of Si is 0.2%.

[0085] The difference between Comparative Example 5 and Example 3 is that the contents of several solid solution elements capable of regulating the carbon corrosion resistance of the nickel-chromium-based alloy material are changed, including Co, Ta, Nb, and Y. The content of Co is 0.3%, the content of Ta is 0.06%, the content of Nb is 0.05%, and the content of Y is 0.5%.

[0086] Table 1 Element contents of nickel-chromium alloy materials in Examples 1 to 8 of the present invention

[0087]

[0088] Test Example 1

[0089] The performance of the nickel-chromium-based alloy heating wires of Examples 1 to 8 and Comparative Examples 1 to 5 was tested, and the specific data are shown in Table 2.

[0090] 1. Resistivity Detection The nickel-chromium-based alloy materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were tested for resistance using a resistance meter. The test results are as follows: Figure 1 shown.

[0091] Result analysis: From Figure 1 It can be seen that the resistance values ​​of Examples 1 to 8 are within the range of 0.6 to 1.0 μΩ·m, and the resistivity can be regulated by changing the composition of the alloy material. This shows that in the actual application of nickel-chromium-based alloy materials, nickel-chromium-based alloy heating wires that meet actual needs can be produced according to actual heating requirements. In Comparative Examples 2 to 3, we changed the resistivity of the alloy heating wire by changing the solid-solution elements that affect the resistivity. It can be seen from the figure that the resistivity of Comparative Examples 2, 3 and 4 has changed greatly. It shows that the content of several solid-solution elements that have an influencing factor on the resistivity of the nickel-chromium-based alloy material heating wire is a key parameter of the present invention.

[0092] 2. Tensile strength test

[0093] The tensile strength of the nickel-chromium-based alloy materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5 was tested using a universal testing machine. The test results are as follows: Figure 2 shown.

[0094] Result analysis: From Examples 1 to 5, it can be found that the tensile strength of the alloy decreases slightly with the decrease of nickel content. In Examples 6 and 7, we can increase the tensile strength of the material by adding elements such as iron, cobalt, tantalum, and yttrium. At the same time, in Comparative Example 1, when we control the content of nickel and chromium outside the range of the present invention, the tensile strength of the material will be seriously reduced. It is proved that the content of the main elements of the present invention and the content of elements such as iron, cobalt, tantalum, and yttrium that can increase the tensile strength of the material are key parameters of the present invention.

[0095] 3. Thermal conductivity test The average thermal conductivity of the nickel-chromium based alloy materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5d was tested using a laser thermal conductivity tester. The results are as follows: Figure 3 shown.

[0096] Result analysis: From Figure 3 It can be seen that the thermal conductivity of Examples 1 to 8 is basically maintained at 20 W·m -1 ·K -1 After changing the contents of the two solid solution elements C and Si in Comparative Examples 3 and 4, the thermal conductivity is greatly reduced. This shows that the contents of the two elements C and Si play a vital role in the resistivity and thermal conductivity of the nickel-chromium-based alloy material. Slight changes in the contents of these two elements will directly affect the performance of the nickel-chromium-based alloy heating wire.

[0097] 4. Carbonate corrosion resistance test The nickel-chromium-based alloy materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were subjected to a medium temperature (400°C) corrosion test using a salt spray test chamber and a carbonate mixture. The corrosion test was carried out for a total of 300 hours. Each group of experiments was then weighed, and the weight gain ratio of the sample was calculated to obtain the relative corrosion rate of the nickel-chromium-based alloy material. The results are shown in FIG. Figure 4 shown.

[0098] Result analysis: From Figure 4 It can be seen that Examples 1 to 8 and Comparative Examples 1 to 4 all exhibit relatively low corrosion rates. In Comparative Example 5, the contents of several corrosion-resistant elements such as tantalum, yttrium, and cobalt were reduced, and it can be found that the corrosion rate of the material increased sharply, indicating that the contents of several carbonate corrosion-resistant elements of the present invention play a key role in the corrosion resistance of the material.

[0099] Table 2 Main performance parameters of Examples 1 to 8 and Comparative Examples 1 to 5

[0100]

[0101] In order to more intuitively reflect the thermal response performance of the nickel-chromium alloy heating wire involved in this patent, the heating speeds of Example 1, Example 5, and Example 8 are compared with the comprehensive performance of other common heating wires on the market (copper wire, iron-chromium-aluminum alloy wire, nickel-chromium alloy wire, chromium-aluminum-niobium alloy wire):

[0102] 1) One alloy wire with a diameter of 1 mm and a length of 1 m was cut from each of Example 1, Example 5, Example 8, copper wire, iron-chromium-aluminum wire, nickel-chromium wire, and chromium-aluminum-niobium wire. Under the same experimental conditions, 220 V AC was passed through the wires. The time taken for the surface temperature of the alloy wires to rise from room temperature (20° C.) to 600° C. was measured using a high-temperature infrared temperature measuring gun. The results are shown in Table 3.

[0103] Table 3 Time taken for various heating wires to heat to 600°C

[0104] Alloy wire type Example 1 Example 5 Example 8 Copper wire Iron-chromium-aluminum Nickel-Chromium Chromium Aluminum Niobium Heating time 1.23s 1.76s 1.51s 2.53s 1.41s 1.65s 1.88s

[0105] 2) The resistivity detection method described above was used to test the resistivity of Example 1, Example 5, Example 8, copper wire, iron-chromium-aluminum wire, nickel-chromium wire, and chromium-aluminum-niobium wire. The specific results are shown in Table 4:

[0106] Table 4 Resistivity of various heating wires

[0107] Alloy wire type Example 1 Example 5 Example 8 Copper wire Iron-chromium-aluminum Nickel-Chromium Chromium Aluminum Niobium Resistivity μΩ·m 0.95 0.75 0.86 0.018 0.91 0.85 0.68

[0108] 3) The relative carbon corrosion rates of Example 1, Example 5, Example 8, copper wire, iron-chromium-aluminum wire, nickel-chromium wire, and chromium-aluminum-niobium wire were tested using the above carbonate corrosion resistance test method. The results are shown in Table 5.

[0109] Table 5 Relative corrosion rate of carbon in various heating wires

[0110] Alloy wire type Example 1 Example 5 Example 8 Copper wire Iron-chromium-aluminum Nickel-Chromium Chromium Aluminum Niobium Relative corrosion rate 3.562 3.986 3.327 8.956 15.623 4.021 4.126

[0111] As can be seen from Tables 3 to 5, the heating wire of Example 1 only takes 1.23 seconds to heat up from room temperature to 600°C, and its resistivity and carbon corrosion resistance are better than those of the currently used mainstream heating wires. Comprehensive comparison. The heating rate, resistivity and carbon corrosion resistance of the nickel-chromium alloy heating wire with multiple elements solid solution provided by the present invention are better than those of the currently used mainstream heating wires, are suitable for working in high temperature and corrosive environments, and can respond quickly to heating and rapid cooling.

[0112] The above is only an embodiment of the present invention, and the common sense such as the known specific component content and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the content of the nickel-chromium-based alloy of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect and practicality of the implementation of the present invention. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A fast-response heating-resistant carbon corrosion-resistant nickel-chromium-based alloy material, characterized in that: The nickel-chromium-based alloy material is composed of the following chemical components in mass percentage: 59% to 81% nickel, 15% to 31% chromium, 0.6% to 6% iron, 0.8% to 1.6% cobalt, 0.05% to 0.12% zirconium, 0.2% to 0.8% manganese, 0.5% to 0.8% tungsten, 0.03% to 0.2% tantalum, 0.1% to 0.5% niobium, 1% to 2.1% yttrium, and 0.02% to 0.08% of 20 to 100 nm silicon carbide nanoparticles.

2. A method for preparing the fast-response heating-resistant carbon corrosion nickel-chromium-based alloy material according to claim 1, characterized in that: To do this, follow these steps: (1) Prepare the chemical composition according to claim 1, mix the raw material powders and dry them in a drying oven at 60°C to 80°C for 15 to 25 hours to obtain a mixed material; (2) The mixed material is placed in a vacuum induction furnace and smelted at 1200°C to 1400°C for 6 to 10 hours under argon protection to obtain the target carbon corrosion-resistant nickel-chromium-based alloy material.

3. A nickel-chromium alloy heating wire prepared from the carbon corrosion-resistant nickel-chromium-based alloy material prepared according to claim 2, characterized in that: The preparation method is as follows: 1) Cutting the nickel-chromium-based alloy material into appropriate lengths, heating it to 800° C., placing it into an extrusion die for extrusion at a pressure of 50-75 MPa and an extrusion speed of 20-30 mm / min; placing the extruded alloy into a drawing die of appropriate size for drawing at a drawing speed of 160-200 mm / min to obtain a nickel-chromium alloy wire of a specified size; 2) The nickel-chromium alloy wire is heated to 500-750° C. and tempered for 2-12 hours. After the tempering is completed, the wire is cooled to room temperature with the furnace to obtain a nickel-chromium alloy heating wire with carbon corrosion resistance and fast response heating.

4. An application of the fast-response heating-resistant nickel-chromium alloy material according to claim 1 in preparing heating elements for electronic cigarettes for atomizing cigarette oil and heating electronic cigarettes for heating solid cigarette particles.

5. Use of the fast-response heating-resistant nickel-chromium alloy material according to claim 1 in preparing thermocouples for measuring high temperatures.

6. Use of the fast-response heating and carbon-corrosion-resistant nickel-chromium alloy material according to claim 1 in preparing a heating element of an electric heating type heater.