A lightweight pile coating steel plate and its production method
Through microalloyation of specific elements and process treatment, steel plates with high corrosion resistance and hydrogen-induced crack resistance are formed, which solves the problem of high-strength steels in the existing technology that cannot meet the corrosion resistance and hydrogen-induced crack resistance in the offshore wind power environment, and achieves the 500MPa level Mechanical-welded-corrosion resistance matching properties of lightweight steel.
Patent Information
- Application Number
- CN202211610433.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-14
AI Technical Summary
The existing technology cannot provide lightweight, corrosion-resistant, and hydrogen-induced crack-resistant steel materials above 460MPa, especially in complex sea areas offshore wind power and other environments. The existing steel materials for hydrogen-induced crack-resistant steel cannot solve the corrosion resistance of steel, which is difficult to Meet the material needs of lightweight structures such as offshore wind power.
Using a steel plate with specific components, containing C, Si, Mn, Mg, Ca, V, N, Cu, Ni, Mo, Re, Ta, Cr, REM, Sn, Sb, Ti, P and other elements, through The addition and synergistic effect of composite trace elements form 70-80% bainite + 15-25% ferrite structure, combined with the precipitation of nanophase, improve the corrosion resistance and hydrogen-induced crack resistance of the steel plate, and adopt high temperature to directly Rolling and low-temperature heating treatment processes to control grain size and distribution of precipitation phases.
The corrosion resistance and hydrogen-induced crack resistance of the steel plate are significantly improved, the yield strength reaches 500~530MPa, the yield strength ratio is ≤0.73, and the elongation is ≥20%. The corrosion resistance is 3.5Ni in the perimeter immersion test of simulated marine seawater splash zone. The system steel is increased by 29-88%, and there is no crack in the environment of 40℃×85% RH, meeting the corrosion performance of NACE A solution for 96 hours.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material preparation, and particularly relates to a coated steel plate for a lightweight pile body and a production method thereof. Background Art
[0002] The offshore wind farm system is huge and expensive, mainly due to the cost of offshore wind power foundation, installation and operation and maintenance of the wind farm. The cost of wind power foundation accounts for about 20% to 30% of the cost of the entire wind farm. As offshore wind farms gradually move from offshore to deep sea and install larger capacity generators, the foundation cost will increase further. The design and research of low-cost foundation structures is the key to reducing the cost of wind turbines. How to reduce foundation costs is one of the key issues that urgently need to be solved in the entire offshore wind power field, and it is also the focus of offshore wind power developers and research institutions.
[0003] High-strength and ultra-high-strength steel can effectively reduce the weight of wind turbine foundations and wind towers, which is not only conducive to ensuring safety, but also can reduce its own weight, welding workload, material transportation costs and increase bearing capacity. At present, offshore wind turbines mainly use structural steel for marine engineering, and the application standard is GB 712-2011 "Structural Steel for Ships and Marine Engineering", with a yield strength of 355MPa, grades DH36 and EH36, and the delivery state is normalized. With the increase in the number of large wind turbines and the increase in the thickness of the steel plates used, and under the pressure of reducing construction costs, offshore wind power plants in Europe, Japan and other countries have begun to use low-alloy steel plates with a yield strength of 460MPa or 500MPa in batches to reduce the thickness of the steel plates while ensuring costs and structural rigidity.
[0004] The invention patent with application number 201710075154.0, "A high corrosion resistant low alloy steel suitable for high temperature coastal environment", the invention patent with application number 201611097512.X, "A high strength weathering steel resistant to high humidity and heat marine atmosphere environment", and the invention patent with application number 201611102046.X, "High strength weathering steel resistant to high humidity and heat marine atmosphere environment and preparation method". All of them adopt high Ni system and alloy with elements such as Cu and Mo. The problem is that the cost is high, and due to the high alloying and carbon equivalent, the welding performance has problems, and the risk of hydrogen induced cracking is not considered. The invention patent with application number 201880084248.7, "Steel with excellent hydrogen induced cracking resistance and manufacturing method", proposes a steel for pressure vessels and its manufacturing method that effectively ensures hydrogen induced cracking (HIC) resistance, but it cannot solve the corrosion resistance of steel under marine environment conditions.
[0005] In summary, existing research is all aimed at improving the corrosion resistance of materials in harsh environments, lacking an overall consideration of H resistance. Existing solutions for steels that resist hydrogen-induced cracking cannot solve the corrosion resistance of steel grades, and lightweight, corrosion-resistant, and hydrogen-induced crack-resistant steel materials with a strength of >460MPa are difficult to meet the material requirements of lightweight structures such as offshore wind power in complex sea areas. In addition, for some extremely harsh coastal construction environments and applications with coating requirements, the local failure and corrosion caused by coating damage and aging are extremely harmful, which is particularly important for the long-term serviceability of the combined use system of steel + coating. Not only does it require good corrosion resistance of steel, but the steel-coating interface system also requires high corrosion resistance.
[0006] Currently, there is no lightweight, hydrogen-resistant special steel with a strength of >460MPa for coating systems that are resistant to harsh marine environments. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to propose a lightweight pile coating steel plate and a production method thereof, which has good comprehensive performance of mechanical-welding-corrosion resistance matching, and a strength of 500MPa level. It can effectively solve problems such as H-induced cracks caused by strength improvement, and has stable service capability under coating.
[0008] In order to solve the above problems, the technical solution adopted by the present invention is as follows: a lightweight steel plate for coating a pile, wherein the steel composition comprises, by weight percentage, C: 0.03-0.06wt%, Si: 0.3-0.45wt%, Mn: 0.7-1wt%, Mg: 0.005-0.01wt%, Ca: 0.008-0.015wt%, V: 0.04-0.06wt%, N: 0.012-0.016wt%, Cu: 0.3-0.5wt%, Ni: 0.005-0.01wt%, Ca: 0.008-0.015wt%, V: 0.04-0.06wt%, N: 0.012-0.016wt%, Cu: 0.3-0.5wt%, Ni: 0.005-0.01wt%, Ca: 0.008-0.015wt%, V: 0.005-0.01wt%, Ni: 0.005-0.01wt%, Cu: 0.005-0.01 ... .8-1.2wt%, Mo: 0.1-0.2wt%, Re: 0.02-0.03wt%, Ta: 0.01-0.02wt%, Cr: 1-1.5wt%, REM: 0.03-0.05wt%, Sn: 0.1-0.2wt%, Sb: 0.05-0.1wt%, Ti: 0.001-0.005wt%, P: 0.01-0.015wt%, S: ≤0.005wt%, the balance is Fe and other inevitable impurities.
[0009] Furthermore, the average grain size of the steel plate 1 / 4-1 / 8 of the thickness is 20-30 μm, the average grain size of the steel plate core is 30-50 μm, and the steel plate contains 70-80% bainite + 15-25% ferrite structure, and the percentages are area percentages.
[0010] Furthermore, the steel plate contains dispersed precipitated V(C, N), Mo2C, TaC, and Fe3C nanophases with an average size of 13-24nm, the average spacing between these precipitated phases is 1.2-2.5μm, and contains Cu nanophases with an average size of 40-55nm, and the average spacing between the phases is 1-2μm.
[0011] Furthermore, the steel plate contains dispersed precipitated V (C, N), Mo2C, TaC, Fe3C nanophases with a size of 10-30nm, and a Cu nanophase with a size of 30-70nm.
[0012] Furthermore, the steel plate has a yield strength of 500-530 MPa, a yield strength ratio of ≤0.73, an elongation of ≥20%, and an impact energy of not less than 170 J at -40°C.
[0013] Furthermore, the HIC corrosion resistance of the steel plate satisfies CSR≤1%, CLR≤1%, and CTR≤1% after 96 hours of NACE A solution corrosion.
[0014] The second technical solution of the present invention is to provide a method for producing a lightweight pile coating steel plate, which is characterized by including smelting, continuous casting, billet heating, controlled rolling and offline processing, and the specific contents are as follows:
[0015] Billet heating: The billet is cold loaded into the furnace at a temperature of ≤80°C, and multi-stage heating is adopted, wherein the total time at 650-950°C is controlled within 0.2-0.3min / mm, the total time at 1210-1230°C is controlled within 0.1min / mm, and the total time at 1170-1210°C is controlled within 0.2-0.4min / mm;
[0016] Controlled rolling: high temperature direct rolling, starting rolling temperature ≥1030℃, first two passes with a reduction rate of 23-35%, average pass reduction rate of 15-22%, final rolling temperature ≥900℃, cooling rate 4-9℃ / s, final cooling temperature 685-730℃;
[0017] Off-line treatment: After the steel plate is air-cooled off the line, the second stage precipitation phase and internal stress are regulated by stacking or insulation treatment, and the insulation regulation temperature is 330-380℃.
[0018] Furthermore, the steel billet is made by converter smelting + continuous casting, and cooling begins when the surface temperature of the steel billet is 830-870°C, and the cooling rate is controlled at 4-11°C / s. Thereafter, low-temperature heating treatment is adopted, and the low-temperature heating temperature is controlled at 200-290°C.
[0019] Furthermore, the steel is smelted in a converter, the Ti element in the molten iron is controlled below 0.005wt%, and Si and Mn are used for deoxidation.
[0020] The coated steel sheet produced according to the above scheme has the following beneficial effects:
[0021] 1. The corrosion resistance of steel plates is greatly improved through the addition and synergistic effect of composite trace elements. Using a simulated ocean seawater splash zone immersion test, under the coating system, the corrosion resistance is improved by 29-88% compared with 3.5Ni system steel;
[0022] 2. It has good comprehensive mechanical properties, structural safety and weldability, with yield strength of 500-530Mpa, yield strength ratio ≤0.73, elongation ≥20%, and impact energy of not less than 170J at -40℃;
[0023] 3. The HIC corrosion resistance meets the requirements of CSR≤1%, CLR≤1%, and CTR≤1% after 96 hours of NACE A solution corrosion;
[0024] 4. There is no crack in the small iron grinding test under 40℃×85%RH environment. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other examples improved or modified by ordinary technicians in this field belong to the scope of protection of the present invention. It should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention.
[0026] The present invention is aimed at the steel materials facing high temperature, unstable oxygen, low pH value, high Cl - In a more complex environment, the pH value of the anode area is reduced through the microalloying and compounding of elements such as Sn, Re, REM, N, V, Cr, W, Ca, and Mg, thereby improving the system potential, reducing the local pH value, and improving the coupled passivation ability of the steel-coating system. The developed steel plate has good comprehensive performance of mechanical-welding type-corrosion resistance matching, and the strength reaches 500MPa level, which can effectively solve the problems of H-induced cracks caused by the increase in strength, and has stable service capability under the coating. Using the simulated ocean seawater splash zone immersion test, the corrosion resistance of the steel plate coating system is 25-90% higher than that of 3Ni system steel.
[0027] The steel composition of the present invention will be described in detail below. Unless otherwise specified, the content of each element is expressed in % by weight.
[0028] The invention discloses a lightweight steel plate for coating a pile body, wherein the steel composition comprises C: 0.03-0.06wt%, Si: 0.3-0.45wt%, Mn: 0.7-1wt%, Mg: 0.005-0.01wt%, Ca: 0.008-0.015wt%, V: 0.04-0.06wt%, N: 0.0012-0.016wt%, Cu: 0.3-0.5wt%, and Ni: 0.8-1.2wt% in terms of weight percentage. , Mo: 0.1-0.2wt%, Re: 0.02-0.03wt%, Ta: 0.01-0.02wt%, Cr: 1-1.5wt%, REM: 0.03-0.05wt%, Sn: 0.1-0.2wt%, Sb: 0.05-0.1wt%, Ti: 0.001-0.005wt%, P: 0.01-0.015wt%, S: ≤0.005wt%, the balance of Fe and other inevitable impurities.
[0029] C: 0.03-0.06wt%
[0030] The C element is the main phase change controlling element for forming a corrosion-resistant structure with 70-80% bainite + 15-25% ferrite as the matrix, and is also an important element for ensuring the strength of the steel. Appropriate C promotes the formation of important tiny cathode phases V (C, N), TaC, and Mo2C in the present invention. These phases help to improve the corrosion resistance of the steel. However, in a high humidity, heat, and high flying salt environment, more C is not conducive to the corrosion resistance and weldability of the steel. Therefore, the C content is 0.03-0.06wt%.
[0031] Si: 0.3-0.45wt%
[0032] The Si element plays a certain role in strengthening and is one of the important deoxidizers of the present invention. It can promote the surface enrichment of Sn and form surface oxides with Cu and Sn, effectively improving the corrosion resistance. Appropriate Si helps to improve the potential of the coating system and control the local pH value, so the Si content is controlled at 0.3-0.45wt%.
[0033] Mn: 0.7-1wt%
[0034] The Mn element plays a certain role in strengthening and is one of the important deoxidizers of the present invention, so the Mn content is controlled to be 0.7-1wt%.
[0035] Ca: 0.008-0.015wt%, Mg: 0.005-0.01wt%
[0036] The Ca and Mg elements are mainly used to reduce the cathode reaction area and the pH value under the coating, which plays a passivation role in protecting Cr; in addition, trace amounts of Ca and Mg dissolved in Fe can make Ni, Cu, Cr, Sn and other corrosion-resistant elements relatively enriched after the surface Fe dissolves in the early stage of corrosion, improve corrosion resistance, and reduce the toughness reduction problem caused by the addition of high Sn and other elements. The above elements will also form a coupling effect with Zn in the primer in a weakly acidic environment to improve the corrosion resistance of the steel-coating system. Based on the above design, the content of Ca and Mg elements is controlled at 0.008-0.015wt% and 0.005-0.01wt%, respectively.
[0037] V: 0.04-0.06wt%
[0038] As an important solid solution and precipitation strengthening element, V element plays an important role in the toughness of steel and is also an important ferrite stabilizing element. The role of V in the present invention is mainly to form V (C, N) with appropriate proportions of C and N. Since the steel material is a multiphase structure formed by multi-element alloying, the control of the cathode ratio in the micro region is very important. The refined, dispersed, uniform and distributed cathode design is very important for controlling the corrosion resistance of the complex structural system of the steel material. Based on this, the present invention adopts a trace amount of 0.04-0.06wt% of V to give full play to its excellent precipitation effect. The electrochemical impedance spectrum shows that after full precipitation, the surface inductive arc of the steel grade is greatly weakened, indicating that the pitting phenomenon is effectively suppressed. It mainly plays the role of controlling the cathode phase. Under the configuration of V, C, N and Cr elements adopted in the present invention, it will promote the generation of 10-30nm dispersed precipitation V (C, N) in the steel matrix, with an average spacing of 1.2-2.5μm, mainly in a spherical shape, which can further prevent the expansion of fatigue cracks. Based on the above design, the content of V is 0.04-0.06wt%.
[0039] N: 0.012-0.016wt%
[0040] The N element mainly promotes the precipitation of fine particles of V (C, N). In addition, the solid-solution N helps to improve the corrosion resistance of the steel and is beneficial to control the ratio of bainite and ferrite. The N in the present invention is controlled at 0.012-0.016wt%.
[0041] Cu: 0.3-0.5wt%
[0042] Cu is an important corrosion resistance and toughening agent of the present invention. In the early stage of corrosion, when the surface is initially corroded, an enrichment layer and an oxide layer are formed, which improves the lack of significant segregation behavior. In addition, a nano phase with an average size of 40-55nm is formed inside the steel plate, and the average spacing between the phases is 1-2μm. After the surface rust layer is destroyed, a large number of fine cathode phases are further formed to form a unique cathode size and distribution control system with V (C, N) and Fe3C, which controls the corrosion rate and helps to improve weldability. However, too much Cu is not conducive to further exertion of corrosion resistance and increases unnecessary costs. Therefore, the Cu of the present invention is controlled at 0.3-0.5wt%.
[0043] Ni: 0.8-1.2wt%
[0044] The main function of Ni element is to balance the toughness of weathering steel. In terms of corrosion resistance, it promotes the positive movement of the self-corrosion potential on the steel surface. The present invention adopts a low Mn component design, so that Ni can more effectively promote the formation of Fe3O4 oxides, and Ni in the rust layer 2+ It can more effectively occupy the interstitial position of Fe3O4, forming a stable and dense intermetallic compound of Fe and Ni, preventing Cl - Diffusion into the matrix reduces acidification and increases the pH value of the electrolyte in the rust layer. Since it is used underwater, Ni is controlled at 0.8-1.2wt%.
[0045] Re: 0.02-0.03wt%
[0046] The Re element is evenly distributed in the dendrite trunk and between dendrites during the solidification process. It is an important solid solution strengthening element. Its corrosion potential is about 0.3V, which can shift the corrosion potential positively, effectively increase the corrosion potential of the matrix, reduce the corrosion current of the system, and improve the corrosion resistance of steel. In addition, an appropriate amount of Re combined with Ni and Cu can effectively promote anode passivation and improve cathode efficiency. Since the anode current in the passivation zone is several orders of magnitude smaller than the current of activation and dissolution, it is very effective to use cathodic elements to improve the corrosion resistance of the alloy. The addition of Re helps to improve the low-temperature and high-temperature stability of the dispersed phases of V and Cu, and improve the bonding between steel and coating. In addition, the compound addition of Re, V, and Ni can effectively control the toughness control problem caused by the addition of elements such as Sn, so it is controlled at 0.02-0.03wt%.
[0047] Ta: 0.01-0.02wt%
[0048] Ta: 0.01-0.02wt%: On the one hand, Ta element shifts the corrosion potential positively by solid solution, effectively increasing the corrosion potential of the matrix, reducing the corrosion current, and thus improving the corrosion resistance of the steel. On the other hand, it forms 10-30nm TaC, which controls the size and shape of the precipitated phase through precipitation and solid solution, and interacts with V and Cu, thereby improving the steel's resistance to hydrogen-induced cracking.
[0049] Mo: 0.1-0.2wt%
[0050] Mo element can make the rust layer dense, and when combined with Si, Cu, etc., the oxide film formed is effective against initial corrosion. In addition, along with the anodic reaction of steel, MoO4 2- Dissolved, MoO4 on the rust layer 2- distribution, producing ion selection, resisting the corrosion promoting factor Cl - Intrusion. In addition, the addition of Mo helps to improve the low and high temperature stability of the V and Cu dispersion phases, improve their pitting resistance, and the precipitated 10-30nm Mo2C complexes with V (C, N), TaC, and Fe3C, which helps to improve the hydrogen-induced cracking ability of steel. Too high is not good for plasticity. In addition, for high-strength steel, Mo can help the toughness of steel, but too much Mo affects the pH value under the coating, which is not conducive to coupling, so it is controlled at 0.1-0.2wt%.
[0051] Cr: 1-1.5wt%
[0052] Cr; on the one hand, it plays the role of dense rust layer, on the other hand, it forms a passive oxide, which together with other oxides and dense α-FeOOH resists Cl - Intrusion; In addition, in the composition design of the multi-component system of the present invention, solid solution elements such as Cr are fully dissolved in the matrix, which reduces the solid solubility of V and improves its precipitation behavior, indirectly controlling the thermodynamic and kinetic changes of V (C, N), and after the compounding of Cr, V and other elements forms a stable rust layer, the inductive effect tends to completely disappear, indicating that the material's pitting resistance has reached the best match. However, too much Cr is not conducive to the control of pH under the coating, so the Cr of the present invention is controlled at 0.5-1wt%.
[0053] REM: 0.03-0.05wt%
[0054] On the one hand, REM rare earth elements can change the size of cathode phases such as V (C\N), increase their dispersion, increase their potential, and reduce their cathode effect. Because the content reaches 0.03-0.05wt%, it is fully dissolved in the matrix, which plays a role in increasing the matrix potential and directly produces corrosion resistance. The REM absorbed by grain boundaries, subgrain boundaries, precipitate mismatches and other positions plays a role in balancing the segregation of elements such as Cr and Cu, reducing intergranular and interphase corrosion caused by segregation.
[0055] Sn: 0.1-0.2wt%
[0056] On the one hand, the Sn element reduces the energy level of steel and weakens the electrochemical activity of steel in the form of a single substance solid solution. In addition, it helps to form oxides such as SnO and deposit on the corrosion front, promotes the formation of α-FeOOH, and compacts the oxide layer together with α-FeOOH. When dissolved together with Fe, the ionic Sn can combine with Cl- to increase the local pH value, especially the pH under the coating, which plays a role in controlling the acceleration of the corrosion process. The Sn content of the present invention is controlled at 0.1-0.2wt%.
[0057] Sb: 0.05-0.1wt%
[0058] The Sb element can improve the ability of steel used underwater to resist local pitting corrosion. According to the requirements of the underwater environment, the Sb content of the present invention is controlled at 0.05-0.1 wt%.
[0059] Ti: 0.001-0.005wt%
[0060] The Ti element helps to control the initial grain size, but too much will consume the N element, affecting the strength and corrosion resistance of the steel. Therefore, the Ti content of the present invention is controlled within 0.001-0.005 wt%.
[0061] P: 0.01-0.015wt%
[0062] The P element is mainly used to reduce the degree of anode polarization, promote the uniform dissolution of steel and accelerate the oxidation rate of iron, promote the formation of non-static protective film, and cooperate with Re, Cu, etc. to resist Cl - Considering that too much P will reduce the weldability of the steel sheet for coating to a certain extent, the P in the present invention is controlled to be 0.01-0.015wt%.
[0063] S: ≤0.005wt%
[0064] S: The sulfide formed by the element accelerates corrosion and reduces the toughness of the steel plate, so it needs to be strictly controlled to ≤ 0.005wt%.
[0065] In addition to the above-mentioned steel components, the balance of the present invention may be Fe and inevitable impurities. Inevitable impurities are impurities that are not artificially mixed in the general steel manufacturing process. They cannot be completely excluded, and the meaning can be easily understood by those skilled in the art of general steel manufacturing. In addition, the present invention does not completely exclude the addition of other components in addition to the above-mentioned steel components.
[0066] The microstructure of the present invention will be described in further detail below.
[0067] The invention discloses a coated steel plate for a lightweight pile body, wherein the steel plate contains a corrosion-resistant structure of 70-80% bainite + 15-25% ferrite, and the percentage is an area percentage. The average grain size of the steel plate 1 / 4-1 / 8 thickness is 20-30 μm, and the average grain size of the steel plate core is 30-50 μm; the steel plate contains dispersed precipitated V (C, N), Mo2C, TaC, Fe3C nanophases, the size of these precipitated phases is 10-30 nm, the average size is 13-24 nm, and the average spacing is 1.2-2.5 μm; the steel plate contains dispersed precipitated Cu nanophases, the size is 30-70 nm, the average size is 40-55 nm, and the average spacing of the phases is 1-2 μm.
[0068] The production process of the present invention is described in further detail below.
[0069] A method for producing a lightweight pile coating steel plate includes smelting, continuous casting, billet heating, controlled rolling and offline processing, and the specific contents are as follows:
[0070] Smelting: The steel is smelted in a converter, and Si and Mn are used for deoxidation. The use of Al is strictly controlled because the addition of Al will consume the N element and have a harmful effect on the surface quality of the steel billet. Similarly, the introduction of the Ti element (Ti≤0.005wt%) in the molten iron must also be strictly controlled to affect the precipitation effect of V and Cu and avoid the formation of Ti, Al and other carbonitrides, which is not conducive to corrosion resistance.
[0071] Continuous casting: The steel billet is made by converter smelting + continuous casting. In order to control the initial surface grain size of the continuous casting billet and the solid distribution of corrosion-resistant elements, rapid cooling is used for pretreatment when the billet is discharged. The billet surface temperature starts to cool at 830-870℃, and the cooling rate is controlled at 4-11℃ / s. After that, it is not suitable for hot loading. Low-temperature heating treatment is required, and the treatment temperature is 200-290℃ to control the surface quality and thermal stress distribution of the billet.
[0072] Billet heating: The temperature of the cold billet in the furnace is controlled at ≤80℃, and multi-stage heating is adopted, where the total time of 650-950℃ is controlled within 0.2-0.3min / mm, the total time of 1210-1230℃ is controlled within 0.1min / mm, and the total time of 1170-1210℃ is controlled within 0.2-0.4min / mm. The purpose is to control the initial distribution of alloy elements and trace elements before hot working. Since the distribution and composition of grains, especially grain boundaries, have a greater impact on corrosion, it is necessary to reasonably control the initial grain size.
[0073] Controlled rolling: The steel plate starts rolling as soon as it leaves the furnace. It is produced by high-temperature direct rolling. The rolling temperature is ≥1030℃, the first two passes have a reduction rate of 23-35%, the average pass reduction rate is 15-22%, and the final rolling temperature is controlled to be ≥900℃. The structure and performance are regulated by controlled cooling. The cooling rate is controlled at 4-9℃ / s. Too fast cooling rate is not conducive to the matching control of toughness and corrosion resistance. The final cooling temperature is 685-730℃. The average grain size of 1 / 4-1 / 8 thickness of the steel plate is controlled at 20-30μm, and the average grain size of the core of the steel plate is controlled at 30-50μm to ensure the strength control of the steel. In addition, the importance of this process is to reduce the control deviation of the precipitation phase caused by the uncontrolled offline thermal history, and to ensure that the components of the main corrosion-resistant elements precipitated in the steel are overcooled to stabilize the precipitation process. In this process, 70-80% bainite + 15-25% ferrite is formed in the steel as the matrix corrosion-resistant structure.
[0074] Off-line treatment: After the steel plates are off the line, they are uniformly stacked and heat-insulated to regulate the second-stage precipitation phase and internal stress. Cooling increases the precipitation dynamics of the fine phase, and low-temperature regulation of 330-380°C can be used. On the one hand, the surface hardness can be regulated and the mechanical properties of the steel plate surface can be improved. On the other hand, finer precipitates are formed to improve the overall corrosion resistance of the steel plate.
[0075] After regulation, dispersed V (C, N), TaC and Mo2C are generated in the matrix of the steel, with a size of 10-30nm and an average size of 13-24nm. These same F3C are compounded and precipitated with an average spacing of 1.2-2.5μm. At the same time, there is also a Cu nanophase in the matrix, with a size of 30-70nm, an average size of 40-55nm, and an average spacing of 1-2μm, which plays a role in controlling the comprehensive performance.
[0076] According to the above chemical composition and production process, the actual smelting composition of the present invention is shown in Table 1, the actual process parameters of the present invention are shown in Tables 2-4, and the actual properties are shown in Tables 5-10.
[0077] Table 1 Composition of each example, wt%
[0078]
[0079]
[0080] Table 2 Pretreatment of blanks
[0081]
[0082] Table 3 Heating process
[0083]
[0084] Table 4 Rolling process and microstructure control results
[0085]
[0086] Table 5 Process technology and organizational proportion level of the billet off-line
[0087]
[0088]
[0089] Table 7 Mechanical properties of the examples
[0090]
[0091] The test steel and the comparison steel were protected by four layers of Zn-rich primer to make accelerated corrosion coupons for coating steel plates. The steel-coating accelerated corrosion test was carried out. The single test method was as follows:
[0092] 1. 42℃, relative humidity 90%, time 5h;
[0093] 2. Accelerated corrosion test simulating sea conditions was adopted, 2% NaCl solution: pH value: PH: 6-6.9, immersion temperature 42±2℃, time 1h;
[0094] 3. Exposure temperature 45±2℃, exposure humidity 60%, time 10h;
[0095] The number of times that 10% coating degradation (peeling of notched parts, bubbling, etc.) occurs after corrosion cycles is used as an evaluation of the corrosion resistance of the system. The number of corrosion cycles is 44 to 64, and the relative corrosion resistance is 129% to 188%.
[0096] Table 8 Corrosion resistance of the examples
[0097]
[0098]
[0099] Table 9 Anti-HIC performance of examples
[0100] Example CLR, % CTR, % CSR, % Test results 1 0 0 0 qualified 2 0 0 0 qualified 3 0 0 0 qualified 4 0 0 0 qualified 5 0 0 0 qualified 6 0 0 0 qualified 7 0 0 0 qualified 8 0 0 0 qualified 9 0 0 0 qualified 10 0 0 0 qualified
[0101] The above embodiments were subjected to the oblique Y-groove welding crack test evaluation (Xiaotieyan test) at 40°C × 85% RH environment. No cracks were found in the dissection results after 48 hours of welding.
[0102] Table 10 Experimental results of the small iron grinder in the embodiment
[0103]
[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A lightweight steel plate for coating piles, It is characterized in that The steel plate composition includes C: 0.03-0.06 wt%, Si: 0.3-0.45wt%, Mn: 0.7-1wt%, Mg: 0.005-0.01 wt%, Ca: 0.008-0.015wt%, V: 0.04-0.06 wt%, N: 0.012-0.016 wt%, Cu: 0.3-0.5wt%, Ni: 0.8-1.2wt%, Mo: 0.1-0.2wt%, Re: 0.02-0.03 wt%, Ta: 0.01-0.02 wt%, Cr: 1-1.5wt%, REM: 0.03-0.05 wt%, Sn: 0.1-0.2wt%, Sb: 0.05-0.1 wt%, Ti: 0.001-0.005 wt%, P: 0.01-0.015 wt%, S: ≤0.005 wt%, the balance is Fe and other unavoidable impurities; The average grain size of the steel plate 1 / 4-1 / 8 thickness is 20-30μm, the average grain size of the steel plate core is 30-50μm, and the steel plate contains 70-80% bainite + 15-25% ferrite structure, and the percentages are area percentages; The steel plate contains V (C, N), Mo with an average size of 13-24nm dispersed precipitation 2 C, TaC, Fe 3 C nanophase, the average spacing of these precipitated phases is 1.2-2.5μm, containing Cu nanophases with an average size of 40-55nm, and the average spacing of Cu nanophases is 1-2μm; Dispersed V (C, N), Mo 2 C, TaC, Fe 3 The size of the C nanophase is 10-30 nm, and the size of the Cu nanophase is 30-70 nm.
2. A lightweight steel plate for coating a pile according to claim 1, It is characterized in that The yield strength of the steel plate is 500-530MPa, the yield strength ratio is ≤0.73, the elongation is ≥20%, and the impact energy at -40℃ is not less than 170J.
3. A lightweight steel plate for coating a pile according to claim 1, It is characterized in that The steel plate's HIC corrosion resistance meets the requirements of CSR≤1%, CLR≤1%, and CTR≤1% after 96 hours of NACE A solution corrosion.
4. A method for producing the lightweight steel plate for coating of piles according to any one of claims 1 to 3, It is characterized in that It includes smelting, continuous casting, billet heating, controlled rolling and offline processing. The specific contents are as follows: Billet heating: The billet is cold loaded into the furnace at a temperature of ≤80°C, and multi-stage heating is adopted, wherein the total time at 650-950°C is controlled within 0.2-0.3min / mm, the total time at 1210-1230°C is controlled within 0.1min / mm, and the total time at 1170-1210°C is controlled within 0.2-0.4min / mm; Controlled rolling: high temperature direct rolling is adopted, the starting rolling temperature is ≥1030℃, the reduction rate of the first two passes is 23-35%, the average reduction rate of the pass is 15-22%, the final rolling temperature is controlled to be ≥900℃, the cooling rate is controlled to be 4-9℃ / s, and the final cooling temperature is 685-730℃; Off-line treatment: After the steel plate is air-cooled off the line, the second stage precipitation phase and internal stress are regulated by stacking or insulation treatment, and the insulation regulation temperature is 330-380℃.
5. The method for producing a lightweight steel plate for coating a pile according to claim 4, It is characterized in that The steel billet is made by converter smelting + continuous casting. The steel billet starts to cool when the surface temperature is 830-870°C, and the cooling rate is controlled at 4-11°C / s. It is then subjected to low-temperature heating treatment, and the low-temperature heating temperature is controlled at 200-290°C.
6. The method for producing a lightweight steel plate for coating a pile according to claim 4, It is characterized in that The steel billet is smelted in a converter, the Ti element in the molten iron is controlled below 0.005wt%, and Si and Mn are used for deoxidation.
Citation Information
Patent Citations
High-strength high dampness and heat sea atmospheric environment resistant weathering resistant steel and preparing method
CN106756476A
High-damp-heat-resistant marine atmosphere high-strength weathering resistant steel
CN106756602A
High-anticorrosion low alloy steel suitable for high-temperature littoral environment
CN106929751A
Steels with excellent resistance to hydrogen-induced cracking and their manufacturing methods
CN111527227B
High-performance steel plate for resisting corrosion of marine splash zone and production method of high-performance steel plate
CN113549819A
Cited By
Lightweight easy-to-process composite transfer printing aluminum plate for semiconductor pattern printing and preparation method of lightweight easy-to-process composite transfer printing aluminum plate
CN122518811A