A method for preparing antibacterial and anticorrosive polyester-nylon ultrafine fiber

By using a mixture of nano-silver particles and nano-zinc oxide particles in polyester and nylon microfibers, combined with blending spinning and stretch setting technology, the problem of insufficient stability of nano-zinc oxide is solved and broad-spectrum antibacterial and long-lasting effects are achieved. The anti-corrosion effect improves the functional durability of the fiber.

CN116288806BActive Publication Date: 2024-10-29ZHEJIANG QINGLAN CHEM FIBER CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310435280.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-29
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

When adding antibacterial and antiseptic effects to existing polyester and nylon microfibers, the dispersion and stability of nano-zinc oxide are weak, resulting in weak functional durability and poor antibacterial and antiseptic effects when made into superfine fiber fillers or long-term textile products. reduce.

Method used

A mixture of nano-silver particles and nano-zinc oxide particles is used as an antibacterial and anti-corrosion material. Through blending spinning technology and stretching and shaping treatment, combined with ultraviolet curing and tea tree extract surface treatment, the anti-bacterial and anti-corrosion properties of the fiber are improved.

Benefits of technology

It achieves broad-spectrum antibacterial and long-lasting antibacterial effects, improves the stability and antibacterial and anti-corrosion properties of the material, and extends the functional durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288806B_ABST
    Figure CN116288806B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing antibacterial and anticorrosive polyester-nylon ultrafine fibers. The invention selects nano silver particles and nano zinc oxide particles as antibacterial and anticorrosive materials. The mixture of the nano silver particles and the nano zinc oxide can produce a synergistic effect to enhance the antibacterial and anticorrosive functions. After stretching and shaping, the prepared ultrafine fibers are cured to improve the antibacterial and anticorrosive properties. The curing method can adopt ultraviolet irradiation, and after the ultraviolet irradiation, the surface is coated with tea tree extract. The tea tree extract contains tea polyphenols, catechins and other ingredients, has anti-oxidation, antibacterial, anti-inflammatory effects and the like, and can be used for the antibacterial and anticorrosive treatment of fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field related to polyester and nylon ultrafine fibers, and in particular to a method for preparing antibacterial and anticorrosive polyester and nylon ultrafine fibers. Background Art

[0002] Polyester microfiber refers to a fiber with a very small diameter made of polyester, generally between 0.1 and 0.5 microns. This kind of microfiber has a wide range of applications due to its high specific surface area and good softness. The main application areas of polyester microfiber include: Filter material: Since the diameter of polyester microfiber is very small, it has excellent filtering performance and can be used to manufacture high-efficiency filtering materials, such as air filters, water treatment filter elements, etc.; Functional textiles: Polyester microfiber can be made into microfiber fabrics, which have good air permeability and comfort, and can be used to manufacture high-end facial cleansing towels, compressed facial masks and other functional textiles; Medical and health products: Polyester microfiber can be made into protective clothing, masks and other medical and health products, which have good protective performance and breathability; Filling materials: Polyester microfiber can be made into microfiber fillers, which have excellent thermal insulation performance and softness, and can be used to manufacture high-end bedding, clothing filling materials, etc.

[0003] Chinese Patent: CN202211176020.5, a nano zinc oxide antibacterial and antiseptic polyester and nylon ultrafine fiber and preparation process, comprising polyester and nylon fiber, imitation ice silk fiber and nano zinc oxide particle gel solution; the intersection of the twisted polyester and nylon fiber and the imitation ice silk fiber is immersed in the nano zinc oxide particle gel solution, and the polyester and nylon fiber and the imitation ice silk fiber are adhered to the nano zinc oxide particle gel solution and then merged to form a polyester and nylon composite fiber, and when the polyester and nylon fiber is processed into a composite fiber, a groove for carrying the nano zinc oxide particle gel solution is set at the merging point of the fiber, so that the merging point is immersed in the nano zinc oxide particle gel solution in the groove, and before twisting and merging, the nano zinc oxide particles are allowed to enter the gap between the two groups of fibers, so that the nano zinc oxide particles are tightly clamped by the two groups of fibers, ensuring that the polyester and nylon fiber after the composite fiber can still guarantee a good antibacterial and antiseptic effect.

[0004] If the polyester-nylon ultrafine fibers in the above patents and prior art need to be enhanced with antibacterial and anticorrosive effects, most of them use the addition of nano zinc oxide particles. However, due to their weak dispersibility and stability, and the low durability of continuous use of a single material, when they are made into ultrafine fiber fillings or some long-term textile products for daily use, their functional durability is weak, resulting in reduced antibacterial and anticorrosive effects. Summary of the invention

[0005] Therefore, in order to solve the above-mentioned shortcomings, the present invention provides a method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme: a method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers, comprising the following steps:

[0007] S1 Raw material selection: polyester fiber and polyamide fiber are used as the main raw materials, and nano silver particles and nano zinc oxide particles are selected as antibacterial and antiseptic materials, wherein the ratio is: for every 100 parts of polyester fiber and polyamide fiber, 18 to 24 parts of nano silver particles and nano zinc oxide particles are selected, and the particle size is 4 to 7 nm;

[0008] Preparation of S2 solution: dissolving the polyester fiber and polyamide fiber in S1 in corresponding organic solvents respectively to form a polyester fiber solution and a polyamide fiber solution; then mixing the nano silver particles and nano zinc oxide particles and adding a surfactant to the two to form an antibacterial and antiseptic mixture; adding the nano silver particles and nano zinc oxide mixture to the polyester fiber solution and stirring in a stirring tank;

[0009] S3 blend spinning: blending the polyester fiber solution containing the antibacterial and antiseptic mixture in S2 with the polyamide fiber solution to form a polymer solution, and using a wet spinning device to produce antibacterial and antiseptic polyester and nylon ultrafine fibers;

[0010] S4 stretching and shaping: the fibers obtained after spinning in S3 are introduced into the stretching and shaping equipment for stretching and shaping, and the auxiliary stretching device A is used to assist the stretching process;

[0011] S5 post-treatment: dyeing and finishing of the fibers after S4 shaping to improve the appearance quality and performance of the fibers;

[0012] S6 performs quality inspection on the antibacterial and antiseptic polyester-nylon microfibers processed in S5, and similarly uses the auxiliary stretching device A to perform stretching inspection on the fibers. The qualified fibers are packaged and prepared for shipment.

[0013] Preferably, the organic solvent in S2 is an ester solvent or a ketone solvent;

[0014] Polyester fiber is dissolved in ester solvent using hot melt method: chop the polyester fiber into pieces, add it to the corresponding organic solvent, heat until dissolved, and stir, the ratio is 1:1.5~2.0; polyamide fiber is dissolved in ketone solvent, also using hot melt method, the ratio is 1:3~4.

[0015] Preferably, the surfactant in S2 is sodium dodecyl sulfate with a concentration of 0.1 mg / mL.

[0016] Preferably, the wet spinning equipment parameter control range described in S3 is: rotation speed: 2000~10000 rpm; electric field strength and direction: 0~10 kV / cm; operating temperature and humidity: 20~35°C and 30%~60%RH; the processing steps are as follows:

[0017] (1) Adding an additive: Adding a salt additive to the polymer solution described in S1 to adjust the surface tension and viscosity of the polymer, the salt additive being 6% to 9%;

[0018] (2) Spinning: injecting the polymer solution to which the salt additive is added in step (1) into a spinner, spraying the solution through the nozzle of the spinner to form fine droplets, which solidify in the air to form nanofibers;

[0019] (3) Fixing the fibers: During the spinning process, the nanofibers in step (2) are deposited and fixed on a collector;

[0020] (4) treating the fibers: post-treating the nanofibers fixed in step (3) to improve the physical and chemical properties of the fibers;

[0021] (5) Collecting fibers: collecting the processed nanofibers.

[0022] Preferably, the stretching and shaping equipment parameters described in S4 are:

[0023] Stretching speed: 0.1~10 mm / min; stretching temperature: 150℃~200℃; stretching ratio: 1~5; setting temperature and time: 10℃~60℃ and 30min~2h; heating rate: less than 10℃ / min; heating method: flow heating.

[0024] Preferably, after the stretching and shaping in S4, the nanofibers are cured, and the curing steps are as follows:

[0025] a. Applying light curing agent: dissolve the light curing agent in a solvent or directly apply it on the fiber surface to fully penetrate into the fiber;

[0026] b. Irradiation with ultraviolet light: placing the fiber coated with the light curing agent under an ultraviolet radiation source for ultraviolet irradiation;

[0027] c Cooling: After UV irradiation, the fiber is cooled to fix its solidification state and shape;

[0028] d. Cutting: Cutting the solidified fibers into the desired fiber shape and length;

[0029] eSurface treatment: The cured microfibers are surface treated and coated with plant extracts.

[0030] Preferably, the plant extract is a tea tree extract, which is coated by roll coating and then dried.

[0031] Preferably, the auxiliary stretching device includes a fixed frame for support, a transmission mechanism arranged at the left end of the fixed frame, a sliding frame installed at the upper end of the fixed frame, guide wheels arranged at the four ends of the sliding frame and attached to the fixed frame, a support plate installed on the top of the sliding frame, support arms fixed at the four ends of the fixed frame, guide rollers installed on the inner side of the support arms for guiding fibers, a support rod installed at the upper end of the fixed frame, and a movable mechanism penetrated by the support rod and connected to the support rod, and guide grooves are opened at the front and rear positions of the upper end of the fixed frame, and four sets of guide wheels are movably embedded in the guide grooves.

[0032] Preferably, the transmission mechanism includes a driving motor arranged at the left end of the fixed frame, a driving pulley connected to the output shaft of the driving motor, a synchronous belt arranged outside the driving pulley, a driven pulley arranged at the other end of the synchronous belt, a transmission shaft installed in the middle of the driven pulley, a swing rod connected to the top of the transmission shaft, a pulling member arranged at the other end of the swing rod, a connecting rod installed on the top of the pulling member, and a pulling rod arranged at the other end of the connecting rod;

[0033] The top of the transmission shaft passes through the shaft seat and is connected to the rocker arm, and the shaft seat is connected to the left side of the fixing frame. The outer side of the pulling member is integrally formed with a connecting rod, and the other end of the connecting rod is hinged to the sliding frame, and the other end of the pulling rod is connected to the moving mechanism.

[0034] Preferably, the moving mechanism includes a bracket penetrated by a support rod, a pulley provided at the upper end of the bracket and in contact with the support rod, a contact plate provided at the bottom of the bracket, and a pulling member connected to the upper and lower ends of the bracket, and the middle part of the left end of the bracket is connected to the pulling rod.

[0035] Beneficial effects of the present invention:

[0036] The present invention uses nano silver particles and nano zinc oxide particles as antibacterial and antiseptic materials.

[0037] The mixture of nano silver particles and nano zinc oxide can produce a synergistic effect and enhance its antibacterial and antiseptic functions. Specifically, the mixed use of nano silver particles and nano zinc oxide can achieve the following effects:

[0038] Broad-spectrum antibacterial: Nano-silver particles and nano-zinc oxide have different bactericidal mechanisms. Mixed use can have antibacterial effects on a wider range of bacteria;

[0039] Long-lasting antibacterial effect: The antibacterial effects of nano-silver particles and nano-zinc oxide can enhance and prolong each other, thus achieving a long-lasting antibacterial effect;

[0040] Improve stability: Since nano-silver particles and nano-zinc oxide have different stabilities, their mixed use can improve the stability of the material and prevent the material from decomposing and failing;

[0041] In addition, a surfactant, sodium dodecyl sulfate, is added to the mixture to increase the dispersibility and stability of the mixture and avoid aggregation and precipitation, which may lead to performance degradation or failure of the mixture.

[0042] The present invention performs a curing treatment on the prepared ultrafine fibers after stretching and shaping to improve their antibacterial and antiseptic properties. The curing treatment method can be ultraviolet irradiation, and after ultraviolet irradiation, the surface is coated with tea tree extract. The tea tree extract contains tea polyphenols, catechins and other ingredients, which have antioxidant, antibacterial, anti-inflammatory and other effects, and can be used for antibacterial and antiseptic treatment of fibers.

[0043] The present invention utilizes an auxiliary stretching device A to assist in the stretching process and the subsequent detection process. An independent motor is installed in the device for driving. The internal transmission mechanism is driven, and the internal pulley group and the connecting rod assembly of the transmission mechanism are driven. The transmission mechanism and the plate inside the moving mechanism can be driven to move relative to each other at the same time, and the left and right relative reciprocating motion is realized to stretch or rub the passing fibers. The present invention has strong stability, reduces manual operation, and effectively improves the efficiency of stretching and the efficiency of subsequent detection work. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a schematic structural diagram of the auxiliary stretching device of the present invention;

[0045] Figure 2 It is a schematic diagram of the transmission mechanism structure of the present invention;

[0046] Figure 3 It is a schematic diagram of the structure of the mobile mechanism of the present invention;

[0047] Figure 4 It is a schematic diagram of the sliding frame structure of the present invention.

[0048] Among them: auxiliary stretching device-A, fixed frame-A1, transmission mechanism-A2, sliding frame-A3, guide wheel-A4, support plate-A4a, support arm-A5, guide roller-A6, support rod-A7, moving mechanism-A8, driving motor-A21, active pulley-A22, synchronous belt-A23, driven pulley-A24, transmission shaft-A25, rocker arm-A26, pulling member-A27, connecting rod-A28, pulling rod-A29, bracket-A81, pulley-A82, contact plate-A83, pulling member-A84. DETAILED DESCRIPTION

[0049] In order to further explain the technical solution of the present invention, it is described in detail below through specific embodiments. Embodiment 1

[0050] The antibacterial and antiseptic polyester-nylon microfiber is made by the following method:

[0051] 100 parts of polyester fiber and 100 parts of polyamide fiber are used, and 18 parts of nano silver particles and nano zinc oxide particles with a particle size of 4nm are selected as antibacterial and antiseptic materials;

[0052] The polyester fiber and the polyamide fiber are dissolved in the corresponding ester solvent and the ketone solvent respectively. The polyester fiber is dissolved in the ester solvent by using the hot melt method: the polyester fiber is chopped, added into the corresponding organic solvent, heated until dissolved, and stirred, and the ratio is 1:1.5; the polyamide fiber is dissolved in the ketone solvent by using the hot melt method, and the ratio is 1:3 to form a polyester fiber solution and a polyamide fiber solution; then the nano-silver particles and the nano-zinc oxide particles are mixed and sodium dodecyl sulfate is added at a concentration of 0.1 mg / mL, and the two are mixed to form an antibacterial and antiseptic mixture; the nano-silver particles and the nano-zinc oxide particle mixture are added to the polyester fiber solution, and stirred in a stirring tank;

[0053] The polyester fiber solution containing the antibacterial and antiseptic mixture and the polyamide fiber solution are blended to form a polymer solution, and the antibacterial and antiseptic polyester-nylon ultrafine fiber is prepared by wet spinning equipment;

[0054] The control range of wet spinning equipment parameters is as follows: rotation speed: 4000 rpm; electric field strength and direction: 5 kV / cm; operating temperature and humidity: 20°C and 30% RH; processing steps: adding salt additives to the polymer solution described in S1 to adjust the surface tension and viscosity of the polymer, and the salt additive is 6%; the polymer solution with the salt additive added is injected into the spinner, and the solution is sprayed out through the nozzle of the spinner to form fine droplets, and the droplets solidify in the air to form nanofibers; during the spinning process, the nanofibers are deposited and fixed on the collector; the fixed nanofibers are post-treated to improve the physical and chemical properties of the fibers; finally, the treated nanofibers are collected.

[0055] The fibers obtained after spinning are introduced into the stretching and shaping equipment for stretching and shaping, and the auxiliary stretching device A is used to assist the stretching process. The parameters of the stretching and shaping equipment are as follows: stretching speed: 5 mm / min; stretching temperature: 150°C; stretching ratio 1:2; shaping temperature and time: 40°C and 1h; heating rate: less than 10°C / min; heating method: flow heating;

[0056] After stretching and shaping, the nanofibers are cured, and the curing steps are: dissolving the photocuring agent in a solvent or directly coating it on the fiber surface to allow it to fully penetrate into the fiber; placing the fiber coated with the photocuring agent under an ultraviolet radiation source for ultraviolet irradiation; irradiating ultraviolet rays: placing the fiber coated with the photocuring agent under an ultraviolet radiation source for ultraviolet irradiation. Ultraviolet irradiation will cause the photoinitiator in the photocuring agent to produce free radicals, causing it to undergo free radical polymerization reaction with the monomers in the polymer, thereby achieving the curing of the fiber; select a suitable ultraviolet light source to control the wavelength and intensity of the ultraviolet light, generally a 365nm wavelength ultraviolet lamp; select a suitable irradiation time to control the intensity and time of the ultraviolet light, which is 5s; select a suitable irradiation distance to control the intensity and depth of the ultraviolet light, which is controlled at 2cm; select a suitable irradiation temperature to avoid thermal decomposition or sintering of the fiber, generally at room temperature; after ultraviolet irradiation, the fiber is cooled to fix its curing state and shape; the cured fiber is cut to prepare the desired fiber shape and length; the cured ultrafine fiber is surface treated and coated with plant extracts; the plant extract is tea tree extract, which is coated by roll coating and dried after coating, and the coated fiber is tested and evaluated, such as antibacterial, antiseptic, washable, wear-resistant and other performance tests to determine the coating effect.

[0057] Dye and finish the shaped fibers to improve their appearance quality and performance;

[0058] The quality of the antibacterial and antiseptic polyester and nylon microfibers is inspected, and the auxiliary stretching device A is used to perform stretching tests on the fibers. The qualified fibers are packaged and prepared for shipment.

[0059] The fiber antibacterial and antiseptic performance testing process includes the following steps:

[0060] Sample preparation: Cut and punch the fiber samples to be tested as required to meet the requirements of the test standards; Bacteria culture: According to the test requirements, select appropriate bacteria, culture, separate, purify and other treatments to obtain pure and active bacteria; Coating treatment: Coat the fiber samples to be tested with plant extract coatings and treat them as required, such as dip coating, spray coating, roll coating, etc.; Antibacterial and anticorrosive performance test: According to relevant standards, the coated fiber samples are contacted with bacteria to conduct antibacterial and anticorrosive performance tests. The test method is: colony counting method, drop the bacterial liquid on the sample surface, culture for a certain period of time, and use a colony counting plate to calculate the number of colonies to evaluate the antibacterial performance of the fiber.

[0061] According to the instruction manual Figure 1-4The auxiliary stretching device A includes a fixed frame A1 for support, a transmission mechanism A2 for driving the entire device is arranged at the left rear end of the fixed frame A1, and the upper right end of the transmission mechanism A2 is respectively connected to the sliding frame A3 and the moving mechanism A8, and a guide groove is provided at the front and rear positions of the upper end of the fixed frame A1, and four groups of guide wheels A4 are movably embedded in the guide groove, and the inner side of the guide wheel A4 is slidably connected with the sliding frame A3, so that the sliding frame moves in the fixed frame A1 along with the guide wheel, and the four ends of the top of the sliding frame A3 are welded with supporting plates A4a through pillars, and the top of the supporting plate A4a faces the moving mechanism A8, and the front and rear positions of the left and right sides of the fixed frame A1 are welded with support arms A5, and the inner sides of the two groups of support arms A5 are rotatably connected with the guide rollers A6, and the guide rollers can conveniently guide the entry and output of the fibers, and two groups of support rods A7 are fixed at the upper end of the back of the fixed frame A1, and the support rods A7 penetrate the moving mechanism A8, and the two are connected, so that the moving mechanism can move on the support rods;

[0062] The transmission mechanism A2 includes a driving motor A21 for driving. The back of the driving motor A21 is fixed to the fixed frame by bolts. The output shaft on the top of the driving motor is connected to the driving pulley A22. The outer side of the driving pulley A22 rotates synchronously with the driven pulley A24 through a synchronous belt A23. The middle of the driven pulley A24 is connected to the transmission shaft A25. The top of the transmission shaft A25 passes through the shaft seat and is connected to the swing rod A26. The shaft seat is bolted to the left side of the fixed frame. The other end of the swing rod A26 is connected to the pulling member A27. The outer side of the pulling member A27 is integrally formed with a connecting rod. The other end of the connecting rod is hinged to the sliding frame A3 to facilitate the pushing of the sliding frame A3. The top of the pulling member A27 is connected to the connecting rod A28. The other end of the top of the connecting rod A28 is hinged to the pulling rod A29. The other end of the pulling rod A29 is connected to the moving mechanism A8, which can drive it stably.

[0063] The moving mechanism A8 includes a bracket A81 for support and penetrated by two groups of support rods A7. Four groups of pulleys A82 are rotatably arranged at the rear end of the bracket A81. The outer sides of the pulleys are in contact with the outer sides of the support rods A7 and can slide on their surfaces. The bracket A81 is L-shaped, and the middle part of the left end of the bracket is hinged to the pulling rod A29 and can be driven by it. A pulling piece A84 is hinged to the upper end of the front end surface of the bracket, and the other end of the pulling piece A84 is hinged to the front end of the top of the bracket. The bottom of the bracket is locked with a contact plate A83 opposite to the top of the support plate A4a.

[0064] The specific implementation process of the auxiliary stretching device A is as follows:

[0065] When the fiber needs to be stretched or tested, it can be guided through the contact plate A83 and the top of the support plate A4a by the guide roller A6, and then guided out by the guide roller A6 at the rear end;

[0066] Then, the driving motor A21 is started to work, and the driving motor drives the driving pulley A22 to rotate, and the transmission shaft A25 in the middle of the driven pulley A24 starts to rotate through the synchronous belt A23, and then acts on the swing rod A26. During the rotation of the swing rod A26, the pulling member and the connecting rod can follow the movement, so that the connecting rod and the connecting rod pull the contact plate A83 and the sliding frame A3 to move respectively;

[0067] During the movement of the sliding frame A3, it can be guided by the guide wheel to move the top support plate A4a, and the contact plate A83 moves through the pulley inside the bracket. The two move relative to each other, and the passing fibers can be pulled and rubbed to the left and right positions, which is convenient for stretching and subsequent detection. Embodiment 2

[0068] The antibacterial and antiseptic polyester-nylon microfiber is made by the following method:

[0069] 100 parts of polyester fiber and 100 parts of polyamide fiber are used, and 24 parts of nano silver particles and nano zinc oxide particles with a particle size of 7nm are selected as antibacterial and antiseptic materials;

[0070] The polyester fiber and the polyamide fiber are dissolved in the corresponding ester solvent and the ketone solvent respectively. The polyester fiber is dissolved in the ester solvent by using the hot melt method: the polyester fiber is chopped, added into the corresponding organic solvent, heated until dissolved, and stirred, and the ratio is 1:2.0; the polyamide fiber is dissolved in the ketone solvent by using the hot melt method, and the ratio is 1:4 to form a polyester fiber solution and a polyamide fiber solution; then the nano-silver particles and the nano-zinc oxide particles are mixed and sodium dodecyl sulfate is added at a concentration of 0.1 mg / mL, and the two are mixed to form an antibacterial and antiseptic mixture; the nano-silver particles and the nano-zinc oxide particle mixture are added to the polyester fiber solution, and stirred in a stirring tank;

[0071] The polyester fiber solution containing the antibacterial and antiseptic mixture and the polyamide fiber solution are blended to form a polymer solution, and the antibacterial and antiseptic polyester-nylon ultrafine fiber is prepared by wet spinning equipment;

[0072] The control range of wet spinning equipment parameters is as follows: rotation speed: 6000 rpm; electric field strength and direction: 10 kV / cm; operating temperature and humidity: 35°C and 60% RH; processing steps: adding salt additives to the polymer solution described in S1 to adjust the surface tension and viscosity of the polymer, and the salt additive is 9%; the polymer solution with the salt additive added is injected into the spinner, and the solution is sprayed out through the nozzle of the spinner to form fine droplets, and the droplets solidify in the air to form nanofibers; during the spinning process, the nanofibers are deposited and fixed on the collector; the fixed nanofibers are post-treated to improve the physical and chemical properties of the fibers; finally, the treated nanofibers are collected.

[0073] The fibers obtained after spinning are introduced into the stretching and shaping equipment for stretching and shaping, and the auxiliary stretching device A is used to assist the stretching process. The parameters of the stretching and shaping equipment are as follows: stretching speed: 8 mm / min; stretching temperature: 200°C; stretching ratio 1:4; shaping temperature and time: 50°C and 1.5h; heating rate: less than 10°C / min; heating method: flow heating;

[0074] After stretching and shaping, the nanofibers are cured, and the curing steps are: dissolving the photocuring agent in a solvent or directly coating it on the fiber surface to allow it to fully penetrate into the fiber; placing the fiber coated with the photocuring agent under an ultraviolet radiation source for ultraviolet irradiation; irradiating ultraviolet rays: placing the fiber coated with the photocuring agent under an ultraviolet radiation source for ultraviolet irradiation. Ultraviolet irradiation will cause the photoinitiator in the photocuring agent to produce free radicals, causing it to undergo free radical polymerization reaction with the monomers in the polymer, thereby achieving the curing of the fiber; select a suitable ultraviolet light source to control the wavelength and intensity of the ultraviolet light, generally a 365nm wavelength ultraviolet lamp; select a suitable irradiation time to control the intensity and time of the ultraviolet light, which is 2s; select a suitable irradiation distance to control the intensity and depth of the ultraviolet light, which is controlled at 1cm; select a suitable irradiation temperature to avoid thermal decomposition or sintering of the fiber, generally at room temperature; after ultraviolet irradiation, the fiber is cooled to fix its curing state and shape; the cured fiber is cut to prepare the desired fiber shape and length; the cured ultrafine fiber is surface treated and coated with plant extracts; the plant extract is tea tree extract, which is coated by roll coating and dried after coating, and the coated fiber is tested and evaluated, such as antibacterial, antiseptic, washable, wear-resistant and other performance tests to determine the coating effect.

[0075] The above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers, Features: The steps include: S1 Raw material selection: polyester fiber and polyamide fiber are used as the main raw materials, and nano silver particles and nano zinc oxide particles are selected as antibacterial and antiseptic materials, wherein the ratio is: for every 100 parts of polyester fiber and polyamide fiber, 18 to 24 parts of nano silver particles and nano zinc oxide particles are selected, and the particle size is 4 to 7 nm; Preparation of S2 solution: dissolving the polyester fiber and polyamide fiber in S1 in corresponding organic solvents respectively to form a polyester fiber solution and a polyamide fiber solution; then mixing the nano silver particles and nano zinc oxide particles and adding a surfactant to the two to form an antibacterial and antiseptic mixture; adding the nano silver particles and nano zinc oxide mixture to the polyester fiber solution and stirring in a stirring tank; S3 blend spinning: blending the polyester fiber solution containing the antibacterial and antiseptic mixture in S2 with the polyamide fiber solution to form a polymer solution, and using a wet spinning device to produce antibacterial and antiseptic polyester and nylon ultrafine fibers; S4 stretching and shaping: the fibers obtained after spinning in S3 are introduced into a stretching and shaping device for stretching and shaping, and an auxiliary stretching device (A) is used to assist the stretching process; S5 post-treatment: dyeing and finishing of the fibers after S4 shaping to improve the appearance quality and performance of the fibers; S6 performs quality inspection on the antibacterial and anticorrosive polyester-nylon microfibers processed in S5, and similarly uses the auxiliary stretching device (A) to perform stretching inspection on the fibers. The qualified fibers are packaged and prepared for shipment; The auxiliary stretching device (A) comprises a fixed frame (A1) for supporting, a transmission mechanism (A2) arranged at the left end of the fixed frame (A1), a sliding frame (A3) installed at the upper end of the fixed frame (A1), guide wheels (A4) arranged at the four ends of the sliding frame (A3) and in contact with the fixed frame (A1), a support plate (A4a) installed at the top of the sliding frame (A3), support arms (A5) fixed at the four ends of the fixed frame, guide rollers (A6) installed on the inner side of the support arms for guiding fibers, a support rod (A7) installed at the upper end of the fixed frame (A1), and a moving mechanism (A8) penetrated by the support rod (A7) and connected to the support rod (A7), wherein a guide groove is provided at the front and rear positions of the upper end of the fixed frame (A1), and four sets of guide wheels (A4) are movably embedded in the guide groove; The transmission mechanism (A2) comprises a driving motor (A21) arranged at the left end of the fixed frame (A1), a driving pulley (A22) connected to the output shaft of the driving motor (A21), a synchronous belt (A23) arranged outside the driving pulley (A22), a driven pulley (A24) arranged at the other end of the synchronous belt (A23), a transmission shaft (A25) installed in the middle of the driven pulley (A24), a swing rod (A26) connected to the top of the transmission shaft (A25), a pulling member (A27) arranged at the other end of the swing rod (A26), a connecting rod (A28) installed at the top of the pulling member (A27), and a pulling rod (A29) arranged at the other end of the connecting rod (A28); The top of the transmission shaft (A25) passes through the shaft seat and is connected to the swing rod (A26), and the shaft seat is connected to the left side of the fixed frame (A1). The outer side of the pulling member (A27) is integrally formed with a connecting rod, and the other end of the connecting rod is hinged to the sliding frame (A3). The other end of the pulling rod (A29) is connected to the moving mechanism (A8); The moving mechanism (A8) comprises a bracket (A81) penetrated by a support rod (A7), a pulley (A82) provided at the upper end of the bracket (A81) and in contact with the support rod (A7), a contact plate (A83) provided at the bottom of the bracket (A81), and a pulling member (A84) connected to the upper and lower ends of the bracket (A81); the middle portion of the left end of the bracket (A81) is connected to the pulling rod (A29).

2. A method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers according to claim 1, Features: The organic solvent in S2 is an ester solvent or a ketone solvent; Polyester fiber is dissolved in ester solvent using hot melt method: chop the polyester fiber, add it to the corresponding organic solvent, heat until dissolved, and stir, the ratio is 1:1.5~2.0; polyamide fiber is dissolved in ketone solvent, also using hot melt method, the ratio is 1:3~4.

3. A method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers according to claim 1, Features: The surfactant in S2 is sodium dodecyl sulfate with a concentration of 0.1 mg / mL.

4. A method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers according to claim 1, Features: The wet spinning equipment parameter control range described in S3 is: rotation speed: 2000~10000 rpm; electric field strength and direction: 0~10 kV / cm; operating temperature and humidity: 20~35℃ and 30%~60%RH; the processing steps are as follows: (1) Adding an additive: Adding a salt additive to the polymer solution described in S1 to adjust the surface tension and viscosity of the polymer, the salt additive being 6% to 9%; (2) Spinning: injecting the polymer solution to which the salt additive is added in step (1) into a spinner, spraying the solution through the nozzle of the spinner to form fine droplets, which solidify in the air to form nanofibers; (3) Fixing the fibers: During the spinning process, the nanofibers in step (2) are deposited and fixed on a collector; (4) treating the fibers: post-treating the nanofibers fixed in step (3) to improve the physical and chemical properties of the fibers; (5) Collecting fibers: collecting the processed nanofibers.

5. A method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers according to claim 1, Features: Parameters of the stretch setting equipment described in S4: Stretching speed: 0.1~10 mm / min; stretching temperature: 150℃~200℃; stretching ratio: 1~5; setting temperature and time: 10℃~60℃ and 30min~2h; heating rate: less than 10℃ / min; heating method: flow heating.

6. A method for preparing antibacterial and antiseptic polyester and nylon ultrafine fibers according to claim 1, Features: After the stretching and shaping described in S4, the nanofibers are cured, and the curing steps are as follows: a. Applying light curing agent: dissolve the light curing agent in a solvent or directly apply it on the fiber surface to fully penetrate into the fiber; b. Irradiation with ultraviolet light: placing the fiber coated with the light curing agent under an ultraviolet radiation source for ultraviolet irradiation; c Cooling: After UV irradiation, the fiber is cooled to fix its solidification state and shape; d. Cutting: Cutting the solidified fibers into the desired fiber shape and length; eSurface treatment: The cured microfibers are surface treated and coated with plant extracts.

7. A method for preparing antibacterial and anticorrosive polyester-nylon ultrafine fibers according to claim 6, Features: The plant extract is a tea tree extract, which is coated by roll coating and then dried.

Citation Information

Patent Citations

  • Nano-zinc oxide antibacterial and anticorrosive polyester-nylon superfine fiber and preparation process thereof

    CN115449942A

  • Antibacterial microfilament composite superfine fiber and preparation method thereof

    CN112779629A

  • Antibacterial polyester-nylon composite fiber and preparation method thereof

    CN114875534A

  • Process of manufacturing core-sheath composite fiber

    EP1600534A1

  • Ultraviolet-curing type coating

    JP1993117547A