A potassium-doped platinum-based catalyst and its preparation method and application
Through the preparation of potassium-doped platinum-based catalysts, nano-titanium dioxide and chloroplatinic acid hexahydrate, combined with potassium nitrate, solve the problem of poor NOx removal effect of supported precious metal catalysts at low temperatures, achieve efficient low-temperature NOx removal, and provide new industrial application ideas.
Patent Information
- Application Number
- CN202310381211.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-11
AI Technical Summary
Existing supported precious metal catalysts have poor denitrification effect in NOx removal at low temperatures, and H2-SCR technology has problems such as NH3 corrosion and escape, CO pollution, etc., making it difficult to meet the demand for efficient NOx removal at low temperatures.
A potassium-doped platinum-based catalyst is used, using nano-titanium dioxide as a carrier material and chloroplatinic acid hexahydrate as a platinum precursor, combined with potassium nitrate, and through stirring, drying, roasting and other steps to prepare a catalyst with a mesoporous structure and highly acidic sites. , used for hydrogen selective catalytic reduction denitration.
The low-temperature NOx removal rate of the catalyst is significantly improved, the activity temperature window is wide, and the NOx degradation rate is as high as 90.29% at 80°C. The preparation process is simple, the materials are cheap and easily available, and it has broad application prospects for low-temperature denitration.
Smart Images

Figure CN116328788B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of air pollution control, and in particular to a potassium-doped platinum-based catalyst and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides (NO x ) mainly refers to nitric oxide (NO) and nitrogen dioxide (NO2), and there are also small amounts of nitrous oxide (N2O) and dinitrogen trioxide (N2O3). Volcanic eruptions and biological activities release a small amount of NO x , while most of NO x Originated from industrial smoke and motor vehicle exhaust. x The elimination of NO is of great significance to the ecological environment and the health of residents. Currently, selective catalytic reduction technology (SCR) is considered to be the most effective way to control NO x The most effective method. SCR technology can be divided into three categories. Among them, NH3-SCR technology is prone to NH3 corrosion and escape, which leads to secondary pollution; CH-SCR technology will produce pollutants such as CO; and H2-SCR has been widely studied and paid attention to due to its advantages of being green and pollution-free and having good low-temperature denitrification activity.
[0003] At present, the catalyst commonly used in H2-SCR reaction is supported precious metal catalyst, and its reaction activity temperature is often between 100-200℃. x The denitrification effect of the removed supported noble metal catalyst at low temperature (<100°C) needs to be further improved. Summary of the invention
[0004] In order to overcome the problems in the prior art, the purpose of the present invention is to provide a potassium-doped platinum-based catalyst and its preparation method and application. The preparation method has the characteristics of simple preparation process, cheap and easy-to-obtain doping materials, high activity at low temperatures, wide active temperature window, etc., and can be used in hydrogen selective catalytic reduction denitrification.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing a potassium-doped platinum-based catalyst, using nano-titanium dioxide as a carrier material, using hexahydrated chloroplatinic acid as a platinum precursor, stirring, drying and calcining the carrier material and the platinum precursor to obtain a platinum-based catalyst;
[0007] The platinum-based catalyst, potassium nitrate and deionized water are mixed, stirred, dried and calcined to prepare a potassium-doped platinum-based catalyst.
[0008] Further, the method specifically includes the following steps:
[0009] (1) dispersing platinum chloride hexahydrate in water to obtain a light yellow transparent clear solution, adding nano titanium dioxide powder, stirring to obtain a microemulsion, and drying and calcining to obtain a platinum-based catalyst;
[0010] (2) Adding a platinum-based catalyst into water to obtain a mixture, adding potassium nitrate particles into the mixture, stirring, drying, and calcining to obtain a potassium-doped platinum-based catalyst.
[0011] Further, the ratio of platinum chloride hexahydrate to water is (0.5-5) g: (50-150) mL.
[0012] Furthermore, the ratio of the light yellow transparent clear solution to the nano titanium dioxide powder is (10-50) mL: (1-5) g.
[0013] Furthermore, in step (1), the drying temperature is 60-90°C and the time is 9-13h; the calcination temperature is 450-550°C and the time is 3-5h.
[0014] Further, the ratio of the platinum-based catalyst to deionized water is 1.8 g: (5-50) mL.
[0015] Further, the ratio of potassium nitrate to the mixture is (0.04-0.2) g: (5-50) mL.
[0016] Furthermore, in step (2), the drying temperature is 60-90°C and the time is 9-13h; the calcination temperature is 450-550°C and the time is 1-3h.
[0017] Application of a potassium-doped platinum-based catalyst prepared by the method as described above in hydrogen selective catalytic reduction denitrification.
[0018] Furthermore, the potassium-doped platinum-based catalyst was fixed in a reactor and nitrogen was introduced at 80°C and a space velocity of 56300 h -1 , H2 volume percentage of 0.4%, O2 volume percentage of 4%, to achieve NO x degradation.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The catalyst prepared by the present invention presents a mesoporous structure. The introduction of potassium enlarges the average pore size of the catalyst, increases the number and strength of acid sites on the catalyst surface, and produces more Pt 0 There is a strong interaction between potassium and the titanium dioxide support, which is not only conducive to improving the catalyst's NO xThe catalyst has a simple preparation process, and the doping materials are cheap and easy to obtain, so it has broad application prospects in the field of low-temperature denitration. The present invention can effectively improve the low-temperature denitration activity and broaden the active window temperature by doping with alkali metal components, which provides a new idea for its further industrial application.
[0021] At 56300h -1 Under the condition of space velocity, high-purity nitrogen, 4% O2, 0.4% H2 and 700ppm NO x When the reaction temperature is only 80°C, the catalyst of the present invention has a great x The degradation rate is as high as 90.29%, realizing hydrogen selective catalytic reduction denitrification. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 N2 adsorption-desorption curves of the catalysts of Examples 1-3 and Comparative Examples of the present invention;
[0023] Figure 2 The pore size distribution curves of Examples 1-3 and the comparative example of the present invention;
[0024] Figure 3 NH3-TPD curves of Examples 1-3 and Comparative Examples of the present invention;
[0025] Figure 4 CO-In situ DRIFTS curves of Examples 1-3 and Comparative Examples of the present invention;
[0026] Figure 5 XRD curves of Examples 1-3 and Comparative Examples of the present invention;
[0027] Figure 6 The activity test curves of the selective catalytic reduction of nitrogen oxides by hydrogen in Examples 1-3 and the comparative example of the present invention are shown. Specific implementation methods
[0028] The present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0029] The invention discloses a method for preparing a potassium-doped platinum-based catalyst, which adopts a step-by-step impregnation method, uses nano-titanium dioxide as a carrier material, uses hexahydrated chloroplatinic acid as a precursor of platinum, and obtains a platinum-based catalyst through stirring, drying, and calcining; then, the platinum-based catalyst, potassium nitrate, and deionized water are mixed, and the mixture is stirred, dried, and calcined to obtain a potassium-doped platinum-based catalyst. The potassium-doped platinum-based catalyst of the invention exhibits excellent low-temperature NO x Removal capability.
[0030] The present invention specifically comprises the following steps:
[0031] (1) Platinum chloride hexahydrate is dispersed in deionized water to obtain a light yellow transparent clear solution, nano titanium dioxide powder is added, and a microemulsion is obtained by a wet impregnation method and magnetic stirring is performed at room temperature (25° C.) for 3-5 hours, which is then dried and calcined to obtain a platinum-based catalyst.
[0032] Wherein, the ratio of solid platinum chloride hexahydrate to water is (0.5-5) g: (50-150) mL;
[0033] The ratio of the light yellow transparent clear solution to the nano titanium dioxide powder is (10-50) mL: (1-5) g.
[0034] The drying temperature is 60-90°C and the time is 9-13h; the calcination temperature is 450-550°C and the time is 3-5h.
[0035] (2) adding the platinum-based catalyst obtained in step (1) into deionized water to obtain a mixture, adding potassium nitrate particles into the mixture, performing a wet impregnation method, magnetically stirring at room temperature for 1-3 hours, drying, and calcining to obtain a potassium-doped platinum-based catalyst.
[0036] Wherein, the ratio of the platinum-based catalyst to deionized water is 1.8 g: (5-50) mL.
[0037] The ratio of potassium nitrate granules to the mixture is (0.04-0.2) g: (5-50) mL.
[0038] The drying temperature is 60-90°C and the time is 9-13h; the calcination temperature is 450-550°C and the time is 1-3h.
[0039] The potassium-doped platinum-based catalyst prepared by the above method is used in hydrogen selective catalytic reduction denitrification, and the application method is: the catalyst is fixed in the middle of the reactor, and the temperature is 80°C and the air velocity is 56300h -1 Under the conditions of 0.4% H2 and 4% O2, potassium-doped platinum-based catalyst achieved 700ppm NO x The maximum conversion rate was 90.29%, which was significantly higher than that of the undoped Pt-based catalyst.
[0040] Example 1
[0041] (1) Dissolve 0.9 g of hexahydrate platinum chloride solid in 100 mL of deionized water to obtain a hexahydrate platinum chloride solution. Measure 2.8 mL of hexahydrate chloroplatinic acid solution and add it to 25 mL of deionized water, stir for 5 min, and obtain a light yellow clear transparent solution. Add 2 g of nano titanium dioxide powder to the above light yellow clear transparent solution, and continue stirring at room temperature at a speed of 400 rpm for 4 h to obtain a microemulsion. Dry the microemulsion at 80°C for 12 h, and calcine it in a muffle furnace at 500°C for 4 h to obtain a platinum-based catalyst, named Pt / TiO2.
[0042] (2) 1.8 g of platinum-based catalyst was added to 22.5 mL of deionized water to obtain a mixed solution. 0.04 g of potassium nitrate was added to the mixed solution, and the mixture was stirred at room temperature for 4 h at a speed of 400 rpm, dried at 80 ° C for 12 h, and calcined in a muffle furnace at 500 ° C for 2 h to obtain a potassium-doped platinum-based catalyst, named 1 wt %K-Pt / TiO2.
[0043] Example 2
[0044] The preparation steps are the same as those of Example 1, except that 0.04 g of potassium nitrate in step (2) of Example 1 is replaced by 0.12 g of potassium nitrate, and the mixture is named 3 wt %K-Pt / TiO2.
[0045] Example 3
[0046] The preparation steps are the same as those of Example 1, except that 0.04 g of potassium nitrate in step (2) of Example 1 is replaced by 0.20 g of potassium nitrate, and the mixture is named 5 wt %K-Pt / TiO2.
[0047] Comparative Example 1
[0048] The Pt / TiO2 catalyst prepared in step (1) of Example 1 was selected.
[0049] The following is a wt %K-Pt / TiO2、3 wt %K-Pt / TiO2、5 wt Taking %K-Pt / TiO2 catalyst as an example, a comparative study was conducted with the Pt / TiO2 catalyst of Comparative Example 1. The specific method and conclusion of the study are as follows:
[0050] Depend on Figure 1 It can be seen that the catalysts of Examples 1-3 and the comparative example exhibit typical type IV adsorption isotherms, indicating that a mesoporous structure exists on the prepared catalysts.
[0051] Depend on Figure 2It can be seen that the pore diameters of the catalysts of Examples 1-3 and the comparative example are in the range of 2-15 nm, and the average pore diameter of Examples 1-3 is larger than that of the comparative example.
[0052] Depend on Figure 3 It can be seen that compared with the comparative example, Examples 1-3 show stronger ammonia desorption peaks at weak acid sites (<200°C), and Examples 2-3 show new ammonia desorption peaks at strong acid sites (>350°C), indicating that potassium doping increases the number and strength of acidic sites on the catalyst.
[0053] Depend on Figure 4 It can be seen that compared with the comparative example, Examples 2-3 show obvious 0 The CO adsorption peak indicates that appropriate K doping can change the valence state of Pt, especially produce more Pt with H2-SCR reaction activity. 0 Species.
[0054] Depend on Figure 5 It can be seen that in Examples 1-3, new KO-Ti diffraction peaks were detected at 2θ=29.72° and 30.72°, indicating that there is a strong interaction between potassium and the carrier titanium dioxide.
[0055] Catalyst activity test:
[0056] The catalysts of Examples 1-3 and the comparative example were tableted and sieved (40-60 meshes), and 0.8 mL of the sieved catalyst was placed in a fixed bed denitration reactor for catalytic activity evaluation. x The initial concentration was controlled at 700ppm, the oxygen concentration was 4%, the H2 concentration was 0.4%, and the reaction space velocity was 56300h -1 The catalysts were tested for NO at 80°C, 100°C, 125°C, 150°C, 175°C and 200°C. x Conversion rate, export NO x The concentration is monitored online by a flue gas analyzer.
[0057] Depend on Figure 6 It can be seen that the potassium-doped platinum-based catalysts of Examples 1-3 exhibited better denitration activity at low temperatures (80-100°C), wherein the potassium-doped platinum-based catalysts of Examples 1-3 had a higher denitration activity for NO at 80°C. x The removal rates of NO were 90.29%, 80.71% and 50.25% respectively. x The removal rate is only 28.14%. x The removal rate is limited, and the catalysts of Example 1 and Example 2 have a wider reaction activity window temperature.
[0058] Example 4
[0059] (1) 0.5 g of platinum chloride hexahydrate is dispersed in 50 mL of deionized water to obtain a light yellow transparent clear solution. 1 g of nano titanium dioxide powder is added to 10 mL of the light yellow transparent clear solution. A microemulsion is obtained by wet impregnation method and magnetic stirring is performed at room temperature (25° C.) for 3 h. The microemulsion is then dried at 60-90° C. for 9-13 h and calcined at 450-550° C. for 3-5 h to obtain a platinum-based catalyst.
[0060] (2) 1.8 g of a platinum-based catalyst was added to 5 mL of deionized water to obtain a mixture, and 0.04 g of potassium nitrate particles was added to 10 mL of the mixture. The mixture was subjected to a wet impregnation method, magnetically stirred at room temperature for 1 hour, dried at 60° C. for 13 hours, and then calcined at 450° C. for 3 hours to obtain a potassium-doped platinum-based catalyst.
[0061] Example 5
[0062] (1) 5 g of platinum chloride hexahydrate was dispersed in 150 mL of deionized water to obtain a light yellow transparent clear solution. 3 g of nano titanium dioxide powder was added to the 50 mL of light yellow transparent clear solution. A microemulsion was obtained by wet impregnation method and magnetic stirring was performed at room temperature (25°C) for 4 hours. The microemulsion was then dried at 70°C for 12 hours and calcined at 550°C for 3 hours to obtain a platinum-based catalyst.
[0063] (2) 1.8 g of a platinum-based catalyst was added to 50 mL of deionized water to obtain a mixture, 0.1 g of potassium nitrate particles was added to the 50 mL mixture, and the mixture was subjected to a wet impregnation method, magnetically stirred at room temperature for 2 h, dried at 70° C. for 12 h, and then calcined at 500° C. for 2 h to obtain a potassium-doped platinum-based catalyst.
[0064] Example 6
[0065] (1) 2 g of platinum chloride hexahydrate was dispersed in 100 mL of deionized water to obtain a light yellow transparent clear solution. 5 g of nano-titanium dioxide powder was added to 20 mL of the light yellow transparent clear solution. A microemulsion was obtained by wet impregnation method and magnetic stirring was performed at room temperature (25°C) for 5 h. The microemulsion was then dried at 80°C for 10 h and calcined at 500°C for 4 h to obtain a platinum-based catalyst.
[0066] (2) 1.8 g of a platinum-based catalyst was added to 10 mL of deionized water to obtain a mixture, and 0.2 g of potassium nitrate particles was added to 30 mL of the mixture. The mixture was subjected to a wet impregnation method, magnetically stirred at room temperature for 3 h, dried at 80° C. for 10 h, and then calcined at 550° C. for 1 h to obtain a potassium-doped platinum-based catalyst.
[0067] Example 7
[0068] (1) 3 g of platinum chloride hexahydrate was dispersed in 70 mL of deionized water to obtain a light yellow transparent clear solution. 4 g of nano titanium dioxide powder was added to 40 mL of the light yellow transparent clear solution. A microemulsion was obtained by wet impregnation method and magnetic stirring was performed at room temperature (25°C) for 3 h. The microemulsion was then dried at 90°C for 9 h and calcined at 470°C for 5 h to obtain a platinum-based catalyst.
[0069] (2) 1.8 g of a platinum-based catalyst was added to 30 mL of deionized water to obtain a mixture, and 0.2 g of potassium nitrate particles was added to 40 mL of the mixture. The mixture was subjected to a wet impregnation method, magnetically stirred at room temperature for 1.5 h, dried at 90° C. for 9 h, and then calcined at 470° C. for 2.5 h to obtain a potassium-doped platinum-based catalyst.
[0070] Example 8
[0071] (1) 4 g of platinum chloride hexahydrate was dispersed in 120 mL of deionized water to obtain a light yellow transparent clear solution. 2 g of nano titanium dioxide powder was added to 30 mL of the light yellow transparent clear solution. A microemulsion was obtained by wet impregnation method and magnetic stirring was performed at room temperature (25°C) for 5 h. The microemulsion was then dried at 65°C for 12 h and calcined at 520°C for 3 h to obtain a platinum-based catalyst.
[0072] (2) 1.8 g of a platinum-based catalyst was added to 35 mL of deionized water to obtain a mixture, and 0.07 g of potassium nitrate particles was added to 20 mL of the mixture. The mixture was subjected to a wet impregnation method, magnetically stirred at room temperature for 2.5 h, dried at 65° C. for 12 h, and then calcined at 530° C. for 1.5 h to obtain a potassium-doped platinum-based catalyst.
[0073] The invention discloses a potassium-doped platinum-based catalyst, a preparation method thereof and application thereof in hydrogen selective catalytic reduction denitration. The catalyst is prepared by a step-by-step impregnation method and has a microporous structure, a larger pore size, a larger number of acidic sites, and a larger number of Pt 0 species, strong metal-carrier interactions, and NO x The catalyst prepared by the present invention has a simple synthesis method, cheap and easy-to-obtain doping materials, good low-temperature reaction activity, a wide active temperature window, and good industrial application prospects.
Claims
1. A method for preparing a potassium-doped platinum-based catalyst, characterized in that: Nano-titanium dioxide is used as a carrier material, hexahydrate chloroplatinic acid is used as a platinum precursor, the carrier material and the platinum precursor are stirred, dried and calcined to prepare a platinum-based catalyst; The platinum-based catalyst, potassium nitrate and deionized water are mixed, dried and calcined after stirring to obtain a potassium-doped platinum-based catalyst; The specific steps include: (1) dispersing platinum chloride hexahydrate in water to obtain a light yellow transparent clear solution, adding nano titanium dioxide powder, stirring to obtain a microemulsion, and drying and calcining to obtain a platinum-based catalyst; (2) adding a platinum-based catalyst to deionized water to obtain a mixture, adding potassium nitrate particles to the mixture, stirring, drying, and calcining to obtain a potassium-doped platinum-based catalyst; The ratio of potassium nitrate to the mixture is (0.04-0.2) g: (5-50) mL; The ratio of platinum-based catalyst to deionized water is 1.8 g: (5-50) mL.
2. The method for preparing a potassium-doped platinum-based catalyst according to claim 1, characterized in that: The ratio of platinum chloride hexahydrate to water is (0.5-5) g: (50-150) mL.
3. The method for preparing a potassium-doped platinum-based catalyst according to claim 1, characterized in that: The ratio of light yellow transparent clear solution to nano titanium dioxide powder is (10-50) mL: (1-5) g.
4. The method for preparing a potassium-doped platinum-based catalyst according to claim 1, characterized in that: In step (1), the drying temperature is 60-90°C and the time is 9-13h; the roasting temperature is 450-550°C and the time is 3-5h.
5. The method for preparing a potassium-doped platinum-based catalyst according to claim 1, characterized in that: In step (2), the drying temperature is 60-90°C and the time is 9-13h; the calcination temperature is 450-550°C and the time is 1-3h.
6. An application of a potassium-doped platinum-based catalyst prepared by the method according to claim 1 in hydrogen selective catalytic reduction denitrification, wherein the potassium-doped platinum-based catalyst is fixed in a reactor, nitrogen is introduced, and the temperature is 80°C and the space velocity is 56300h -1 , H2 volume percentage of 0.4%, O2 volume percentage of 4%, to achieve NO x degradation.
Citation Information
Patent Citations
Novel nitrogen oxide storage and reduction catalyst for exhaust gas purification of lean burn gasoline engine or diesel engine
CN101722010A