Method for preparing degradable polyester based on solvent-free polymerization of 10-undecenoic acid

By reacting 10-undecanoic acid with polyol in solvent-free conditions, and polymerizing with 1,2-ethylenedithiol, the problems of high temperature, high pressure and low yield in traditional methods are solved. It realizes efficient and green aliphatic polyester synthesis, meeting the requirements of green environmental protection and high performance.

CN116333314BActive Publication Date: 2024-11-05SOUTH CHINA UNIV OF TECH
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202310388188.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-11-05
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

The traditional method of preparing polyester using 10-undecanoic acid has problems with the use of organic solvents, high temperature and high pressure conditions, complex steps and low yields, which hinders the application of renewable resources in polymer materials.

Method used

Dienyl ester monomer is prepared by reacting 10-undecanoic acid and polyol under mild conditions under solvent-free conditions, and polymerization is carried out using 1,2-ethylenedithiol to achieve efficient and green aliphatic polyester. synthesis.

Benefits of technology

It achieves high yield, simple process and good performance of polyester, and reduces its dependence on petroleum resources, meets the requirements of green and environmental protection, has mild polymerization conditions and is easy to promote in industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116333314B_ABST
    Figure CN116333314B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing degradable polyester by solvent-free polymerization based on 10-undecenoic acid. Diene ester monomers are prepared using plant oil-based unsaturated fatty acids and polyols as raw materials, and 1,2-ethanedithiol is used as a chain extender to achieve bulk polymerization of diene ester monomers under mild conditions without solvent. The raw material sources for preparing polyesters of the present invention are wide, renewable, simple in process, and high in yield, and are suitable for large-scale industrial production. The polyester material prepared by the present invention has good performance, and its performance can be comparable to that of polyesters based on petroleum raw materials, and it has the possibility of large-scale production. And the polyester is biodegradable, will not cause environmental pollution, and meets the requirements of green environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of renewable resource utilization and green synthesis, and in particular to a method for preparing degradable polyester based on polymerization of 10-undecenoic acid under solvent-free conditions. Background Art

[0002] Polyester is usually a general term for polymers obtained by polycondensation of polyols and polyacids or polymerization of ester monomers. It is a type of engineering plastic with excellent performance and wide applications. It can be made into films and fibers and is widely used in packaging, electronics, medical care, construction, automobiles and other fields. However, high-molecular polyester materials derived from petroleum-based chemicals are typical white pollution materials. They are difficult to degrade under natural conditions and cause serious environmental pollution. Moreover, with the depletion of energy and resources, especially after the oil crisis in the 1970s, people have realized the danger of organic chemical raw materials being completely dependent on non-renewable resources. Therefore, it is particularly important to use renewable resources and adopt green synthesis technology to synthesize degradable polyester materials to reduce dependence on non-renewable resources and pollution to the environment from the source.

[0003] 10-Undecenoic acid is a product of high-temperature cracking of castor oil. It has a wide source and is renewable. Whether from the perspective of environmental protection or sustainable resource utilization, the development of a green synthesis process based on 10-Undecenoic acid has very important practical significance. However, the traditional method of preparing polyester using 10-Undecenoic acid has many defects, mainly manifested in: a variety of organic solvents are used in the reaction process, the reaction conditions are not mild enough, the separation process is cumbersome, the yield is low, and some toxic and expensive reagents are used, which ultimately seriously hinders the application of renewable resources in polymer materials.

[0004] Chinese patent CN103467726A discloses a method for preparing a degradable polyester based on 10-undecenoic acid and vanillic acid. The patent uses plant oil-based unsaturated fatty acids and vanillic acid as raw materials, uses n-butyl titanate as a catalyst, and realizes bulk polymerization under high temperature and high vacuum conditions. The steps are as follows: 1) preparing 11,11′-(ethyl-1,2-dithio)diundecene-1-ol from 10-undecenoic acid; 2) preparing dimethyl vanillate from methyl vanillate; 3) preparing degradable polyester from 11,11′-(ethyl-1,2-dithio)diundecene-1-ol and dimethyl vanillate. However, the patent technology has the following shortcomings: (1) organic reagents such as THF and DMF and multiple catalysts are involved and used in the monomer preparation process; (2) the preparation of degradable polyester is carried out under high temperature and vacuum conditions, which has high requirements on equipment; (3) the entire technical process is relatively complicated and has many reaction steps. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a degradable aliphatic polyester based on 10-undecenoic acid under solvent-free conditions in order to solve the above-mentioned problems. The method has a simple synthesis process, mild reaction conditions, is green and environmentally friendly, has a high polyester yield, and has good performance. In addition, the raw material source is wide, renewable, green and sustainable, and is easy to promote industrialization.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids and polyols as raw materials to prepare diene ester monomers, using 1,2-ethanedithiol as a chain extender, and realizing bulk polymerization of diene ester monomers under mild conditions without solvents, the specific steps are as follows:

[0008] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0009] 10-undecenoic acid is mixed with a polyol, and stirred at 120-160°C for 15-30 minutes under nitrogen. p-Toluenesulfonic acid is slowly added to continue the reaction until no more water is produced. After the reaction is completed, all the liquid is transferred to a separatory funnel, and washed with a saturated sodium bicarbonate solution for 3 times. The organic phase is then washed with ultrapure water until the lower aqueous phase of the separatory funnel is clear and transparent. After separating the organic phase, it is dried with anhydrous sodium sulfate for 12-24 hours, and filtered to obtain the target diene ester monomer;

[0010] (2) Preparation of polyester from diene ester monomers

[0011] Add diene ester monomer and 2,2-azobisisobutyronitrile into a three-necked flask and stir in an oil bath at 50-80°C for 15-30 minutes, then add 1,2-ethanedithiol into the three-necked flask for polymerization for 6-12 hours. After the reaction is completed, add methanol solution into the three-necked flask to produce white precipitate, filter and wash the precipitate with ultrapure water, and freeze-dry to obtain white powder, which is the vegetable oil-based aliphatic polyester.

[0012] Furthermore, the raw material 10-undecenoic acid can be produced from plant oil-based unsaturated fatty acids such as oleic acid, ricinoleic acid, ricinoleic acid methyl ester or 10-undecenoic acid methyl ester.

[0013] Furthermore, the polyol includes ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, glycerol, and the like.

[0014] Furthermore, the molar ratio of 10-undecenoic acid to the polyol is 2:1 to 3:1.

[0015] Furthermore, the amount of p-toluenesulfonic acid used is 0.5 to 1.5 wt % of 10-undecenoic acid.

[0016] Furthermore, the molar ratio of the diene ester monomer to 1,2-ethanedithiol is 1:1 to 1:2.

[0017] Furthermore, the amount of 2,2-azobisisobutyronitrile used is 0.5 to 1.0 wt % of the diene ester monomer.

[0018] Furthermore, in step (2), the polymerization reaction temperature is 50 to 80°C.

[0019] Furthermore, in step (2), the ratio of the polymerization product to the methanol solution is 1 g:20 mL.

[0020] Furthermore, the methanol solution is a mixed solution of methanol and water, and the volume ratio of methanol to water is 1:1.

[0021] The vegetable oil-based aliphatic polyester obtained by the above preparation method has a yield of 70% to 85%.

[0022] The present invention uses 10-undecenoic acid derived from vegetable oil and polyols to synthesize diene ester monomers, and then uses 1,2-ethanedithiol chain extension to produce thiol-ene addition polymerization to prepare vegetable oil-based polyester. The polymerization process is carried out under mild conditions and does not require high temperature and high pressure; and the entire reaction process is simple to operate and does not require the use of organic reagents, thereby achieving green preparation of vegetable oil-based polyester. The polyester prepared by the present invention has a yield of up to 85%, and its long-chain aliphatic structure is easily hydrolyzed and microbially degraded in the natural environment, and its thermodynamic properties and thermal stability are comparable to those of commercial degradable plastics.

[0023] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows:

[0024] (1) The raw material for preparing the polyester of the present invention is 10-undecenoic acid, a high temperature cracking product of castor oil. The raw material has a wide source and is renewable, which can reduce the dependence on petroleum resources from the source.

[0025] (2) The polyester synthesis process provided by the present invention is simple, mild in conditions, easy to operate, and green and sustainable, meeting the environmental protection requirements in industrial production.

[0026] (3) The polyester provided by the present invention has a high yield and good polyester material performance, which is comparable to that of polyester based on petroleum raw materials and has the possibility of large-scale production.

[0027] (4) The polyester prepared by the present invention is biodegradable, does not cause environmental pollution, and meets the requirements of green environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is the NMR of 10-undecenoic acid, diene ester monomer and polyester 1 H spectrum.

[0029] Figure 2 It is the infrared spectrum of 10-undecenoic acid, diene ester monomer and polyester.

[0030] Figure 3 This is the DSC curve of the polyester prepared in Example 6.

[0031] Figure 4 This is the thermogravimetric curve of the polyester prepared in Example 6. DETAILED DESCRIPTION

[0032] The following examples are given to specifically illustrate the present invention. It should be pointed out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential adjustments and improvements made to the present invention by ordinary personnel related to this field, including the use of other types of vegetable oil-based unsaturated fatty acids, such as oleic acid, ricinoleic acid, ricinoleic acid methyl ester or 10-undecenoic acid methyl ester to synthesize vegetable oil-based polyesters, still fall within the scope of protection of the present invention.

[0033] Embodiment 1:

[0034] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0035] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0036] 10-undecenoic acid and ethylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid (in an amount of 1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 12 h, and filtered to obtain the target product;

[0037] (2) Preparation of polyester from diene ester monomers

[0038] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 80% to 83%. The average molecular weight (Mw) of the obtained degradable polyester is 6.7 kDa, and the chemical structure is:

[0039]

[0040] Embodiment 2:

[0041] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0042] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0043] 10-undecenoic acid and 1,3-propylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid (in an amount of 1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 12 h, and filtered to obtain the target product;

[0044] (2) Preparation of polyester from diene ester monomers

[0045] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 78% to 82%. The average molecular weight (Mw) of the obtained degradable polyester is 10.9 kDa, and the chemical structure is:

[0046]

[0047] Embodiment 3:

[0048] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0049] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0050] 10-undecenoic acid and 1,4-butanediol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid (in an amount of 1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 12 h, and filtered to obtain the target product;

[0051] (2) Preparation of polyester from diene ester monomers

[0052] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 75% to 78%. The average molecular weight (Mw) of the obtained degradable polyester is 15.9 kDa, and the chemical structure is:

[0053]

[0054] Embodiment 4:

[0055] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0056] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0057] 10-undecenoic acid and 1,6-hexanediol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid (in an amount of 1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 12 h, and filtered to obtain the target product;

[0058] (2) Preparation of polyester from diene ester monomers

[0059] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 77% to 80%. The average molecular weight (Mw) of the obtained degradable polyester is 18.7 kDa, and the chemical structure is:

[0060]

[0061] Embodiment 5:

[0062] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0063] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0064] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 120°C with nitrogen for 30 min, and p-toluenesulfonic acid (0.5 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0065] (2) Preparation of polyester from diene ester monomers

[0066] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 70% to 75%. The average molecular weight (Mw) of the obtained degradable polyester is 52.7 kDa, and the chemical structure is:

[0067]

[0068] Embodiment 6:

[0069] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0070] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0071] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C for 15 min under nitrogen, and p-toluenesulfonic acid (1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0072] (2) Preparation of polyester from diene ester monomers

[0073] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 82% to 85%. The average molecular weight (Mw) of the obtained degradable polyester is 59.4 kDa, and the chemical structure is:

[0074]

[0075] Embodiment 7:

[0076] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0077] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0078] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 160°C for 15 min under nitrogen, and p-toluenesulfonic acid (1.5 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0079] (2) Preparation of polyester from diene ester monomers

[0080] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 80% to 85%. The average molecular weight (Mw) of the obtained degradable polyester is 57.2 kDa, and the chemical structure is:

[0081]

[0082] Embodiment 8:

[0083] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0084] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0085] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C for 15 min under nitrogen, and p-toluenesulfonic acid (1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0086] (2) Preparation of polyester from diene ester monomers

[0087] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (0.5 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 6 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 75% to 78%. The average molecular weight (Mw) of the obtained degradable polyester is 54.3 kDa, and the chemical structure is:

[0088]

[0089] Embodiment 9:

[0090] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0091] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0092] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 3:1, stirred at 140°C for 30 min under nitrogen, and p-toluenesulfonic acid (1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0093] (2) Preparation of polyester from diene ester monomers

[0094] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 70°C oil bath for 30 min. Add 1,2-ethanedithiol (0.02 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 82% to 85%. The average molecular weight (Mw) of the obtained degradable polyester is 58.1 kDa, and the chemical structure is:

[0095]

[0096] Embodiment 10:

[0097] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0098] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0099] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid (in an amount of 1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0100] (2) Preparation of polyester from diene ester monomers

[0101] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in a 50°C oil bath for 30 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 82% to 85%. The average molecular weight (Mw) of the obtained degradable polyester is 54.9 kDa, and the chemical structure is:

[0102]

[0103] Embodiment 11:

[0104] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0105] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0106] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid (in an amount of 1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0107] (2) Preparation of polyester from diene ester monomers

[0108] Diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) were added to a three-necked flask and stirred in a 60°C oil bath for 30 min. 1,2-ethanedithiol (0.01 mol) was added to the three-necked flask and the reaction was continued for 12 h. After the reaction was completed, methanol solution was added to the three-necked flask to produce a white precipitate. The precipitate was filtered and washed with ultrapure water. After freeze drying, a white powder was obtained, which was polyester with a yield of 82% to 85%. The average molecular weight (Mw) of the obtained degradable polyester was 55.7 kDa, and the chemical structure was:

[0109]

[0110] Embodiment 12:

[0111] A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, using plant oil-based unsaturated fatty acids as raw materials and 2,2-azobisisobutyronitrile as a catalyst, and realizing bulk polymerization under mild, solvent-free conditions, the steps are as follows:

[0112] (1) Preparation of diene ester monomer from 10-undecenoic acid

[0113] 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid (in an amount of 1.0 wt% of 10-undecenoic acid) was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent, and the organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product;

[0114] (2) Preparation of polyester from diene ester monomers

[0115] Add diene ester monomer (0.01 mol) and 2,2-azobisisobutyronitrile (1.0 wt% of diene ester monomer) into a three-necked flask and stir in an oil bath at 80°C for 15 min. Add 1,2-ethanedithiol (0.01 mol) into the three-necked flask and continue to react for 12 h. After the reaction is complete, add methanol solution into the three-necked flask to produce a white precipitate. Filter and wash the precipitate with ultrapure water. After freeze drying, a white powder is obtained, which is polyester with a yield of 82% to 85%. The average molecular weight (Mw) of the obtained degradable polyester is 55.8 kDa, and the chemical structure is:

[0116]

[0117] Table 1 Average relative molecular weight distribution of polyester

[0118]

[0119]

[0120] As shown in Table 1, 10-undecenoic acid obtained polyester materials with different molecular weights under different synthesis process conditions. Among them, as the carbon atoms of the diol increased, the molecular weight of the obtained polyester gradually increased, and the propylene glycol with side chain groups was more conducive to the polymerization reaction and increased the molecular weight of the polyester. The molecular weight of the polyester obtained under the best process conditions reached 59.4kDa, which is comparable to some commercial plastics.

[0121] Figure 1 The NMR of 10-undecenoic acid, diene ester monomer and polyester (Example 6) is 1 H spectra, it can be seen that the diene ester monomer and polyester were successfully prepared. After the reaction of 10-undecenoic acid with polyols, the characteristic H spectrum peak of the carboxylic acid disappeared, and the characteristic peak of the ester bond appeared, indicating that the diene ester monomer was successfully prepared; after the reaction of the diene ester monomer with 1,2-ethanedithiol, the characteristic H spectrum peak of the carbon-carbon double bond disappeared, and the characteristic peak of the carbon-sulfur bond appeared, indicating that the plant oil-based polyester was successfully prepared.

[0122] Figure 2 This is an infrared spectrum of 10-undecenoic acid, diene ester monomer and polyester (Example 6), from which it can be seen that the diene ester monomer and polyester were successfully prepared. After 10-undecenoic acid reacts with polyol, the carboxyl group disappears, and the characteristic peak of the ester group appears, indicating that the diene ester monomer is successfully prepared; after the diene ester monomer reacts with 1,2-ethanedithiol, the characteristic absorption peak of the carbon-carbon double bond disappears, and the characteristic absorption peak of the carbon-sulfur bond appears, indicating that the vegetable oil-based polyester is successfully prepared.

[0123] Figure 3 This is the DSC curve of the polyester prepared in Example 6. It can be seen that the glass transition temperature of the polyester is -18.4°C, which is similar to most degradable polymers. The polyester has three melting temperatures (51.2°C, 71.0°C, 77.2°C) and three crystallization temperatures (11.8°C, 41.2°C, 47.4°C), indicating that the obtained polyester is a mixture of three different molecular weights and has a low processing temperature. The main product structural formula is related to the molar ratio of glycerol and 10-undecenoic acid. The three alcohol hydroxyl groups of glycerol can all undergo esterification reaction with the carboxyl group of 10-undecenoic acid to form an ester bond. The product after the reaction is a mixture of three compounds, that is, 1, 2 and 3 10-undecenoic acids are connected to glycerol respectively. When the molar ratio of 10-undecenoic acid to glycerol is 2:1, the product mainly exists in the structure of Example 6; when the molar ratio of 10-undecenoic acid to glycerol is 3:1, the product mainly exists in the structure of Example 9.

[0124] Figure 4 is the thermogravimetric curve of the polyester prepared in Example 6. It can be seen that the mass loss temperature (T 5%a ) appears at 332℃, and the maximum weight loss rate corresponds to the temperature (T d b ) appears at 378°C, indicating that the thermal stability of polyester is similar to that of petroleum-based polymer materials. In addition, the mass residual rate of polyester after heating to 600°C is only 2.3%, indicating that polyester has excellent degradation ability.

Claims

1. A method for preparing a degradable polyester based on 10-undecenoic acid by solvent-free polymerization, characterized in that: The following steps are involved: (1) Preparation of diene ester monomer from 10-undecenoic acid 10-undecenoic acid and propylene glycol were mixed in a molar ratio of 2:1, stirred at 140°C with nitrogen for 15 min, and p-toluenesulfonic acid in an amount of 1.0 wt% of 10-undecenoic acid was slowly added to continue the reaction until no more water was produced. After the reaction was completed, all the liquid was transferred to a separatory funnel, washed with a saturated sodium bicarbonate solution for 3 times, and the organic phase was washed with ultrapure water until the lower aqueous phase of the separatory funnel was clear and transparent. The organic phase was separated and dried with anhydrous sodium sulfate for 24 h, and filtered to obtain the target product; (2) Preparation of polyester from diene ester monomers 0.01 mol of diene ester monomer and 2,2-azobisisobutyronitrile in an amount of 1.0 wt% of diene ester monomer were added to a three-necked flask and stirred in an oil bath at 70°C for 15 min. 0.01 mol of 1,2-ethanedithiol was added to the three-necked flask and the reaction was continued for 12 h. After the reaction was completed, methanol solution was added to the three-necked flask to produce a white precipitate. The precipitate was filtered and washed with ultrapure water. After freeze-drying, a white powder was obtained, which was polyester with a yield of 82% to 85%. The average molecular weight Mw of the obtained degradable polyester was 59.4 kDa, and the chemical structure was as follows: 。

Citation Information

Patent Citations

  • Preparation method for degradable polyester from 10-undecenoic acid and vanillic acid

    CN103467726A

  • Method for preparing hyperbranched polyester

    CN102010504A

  • Method for preparing polyester through using 10-hendecenoic acid and vanillic acid

    CN103319704A

  • Preparation method of cardanol-base polyalcohols and polyurethanes thereof

    CN104086743A

  • Pure plant oil based UV curable prepolymer

    CN104211931A