Compound, rubber mixture containing the compound, vehicle tire having at least one component comprising the rubber mixture, method for preparing the compound and use of the compound as ageing protection agent and / or antioxidant and / or antiozonant and / or dye
By using the compound N-(1,3-dimethylbutyl)-N'-para-hydroxy-p-phenylenediamine as an aging stabilizer, the problem of oxidation reaction of vehicle tires and industrial rubber products under high temperature conditions was solved, and the problem of oxidation reaction of vehicle tires and industrial rubber products was significantly improved. Improves the durability and oxidation resistance of the material.
Patent Information
- Application Number
- CN202180066768.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-02
- Filing Date
- 2021-09-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-09-29
AI Technical Summary
Existing vehicle tires and industrial rubber products are prone to oxidation reactions under long-term storage and high temperature conditions, resulting in material aging and degradation of characteristics. In some cases, existing aging stabilizers have limited protection effects.
The compound N-(1,3-dimethylbutyl)-N'-p-hydroxy-p-phenylenediamine with formula I) is used as an aging stabilizer, through which the enhanced reactivity is enhanced with oxygen, ozone or free radicals. Removal capability, improve the durability and protection of rubber products.
This compound significantly improves the reaction capacity of rubber products to oxygen, ozone and free radicals, extends the durability and antioxidant properties of the material, and shows better protection effects in applications in oils and lubricants.
Smart Images

Figure CN116348311B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a compound, a rubber mixture containing the compound, a vehicle tire comprising the rubber mixture in at least one component, a process for preparing the compound and the use of the compound as an ageing agent and / or antioxidant and / or antiozonant and / or dye. Background Art
[0002] Vehicle tires and industrial rubber articles are known to employ polymeric materials such as, among others, rubber.
[0003] In the case of long-term storage, and especially in target applications that are usually at high temperatures, natural rubber and synthetic polymers (such as IR, BR, SBR, ESBR, etc.), as well as natural and synthetic oils, fats and lubricants, undergo oxidation reactions, which have an adverse effect on the originally desired properties. Depending on the type of polymer, the polymer chains are shortened until the material liquefies or subsequently hardens.
[0004] Therefore, aging stabilizers play a decisive role in the durability of vehicle tires and other industrial rubber products.
[0005] Known aging stabilizers are aromatic amines, for example 6-PPD (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine), IPPD (N-isopropyl-N'-phenyl-p-phenylenediamine) or SPPD (N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine).
[0006] These molecules can react with oxygen or ozone or with the free radicals formed (such as alkyl, alkoxy and alkyl peroxide radicals) and thus scavenge these and thus protect the rubber etc. from further oxidation reactions.
[0007] Weathering stabilizers that are particularly reactive with ozone and effectively scavenge it are also known as "antiozonants." Summary of the invention
[0008] It is an object of the present invention to provide novel compounds which can be used in particular as ageing stabilizers in vehicle tires or other industrial rubber products, thereby achieving an improved protective effect for these products over the prior art.
[0009] This object is achieved by a compound according to the invention as claimed in claim 1, by a rubber mixture according to the invention containing the compound and by a vehicle tire according to the invention comprising the rubber mixture according to the invention in at least one component. The object is further achieved by a process for preparing the compound and by the use of the compound as an ageing stabilizer and / or antioxidant and / or antiozonant.
[0010] The compound according to claim 1 can further be used as a dye.
[0011] The compound according to claim 1 has the formula I):
[0012]
[0013] Thus, the compound of formula I) is N-(1,3-dimethylbutyl)-N′-p-hydroxyphenyl-p-phenylenediamine.
[0014] Compared to the known aging stabilizers 6PPD or IPPD, compounds of formula I) can exhibit an increased reactivity towards oxygen, ozone or free radicals (see above) due to the hydroxyl groups, so that compounds of formula I) achieve an improved protective effect, in particular in vehicle tires and other technical rubber products, as well as in oils and lubricants.
[0015] However, the present invention should not be limited to a specific mechanism of action or a specific explanation.
[0016] DE 1220124 discloses compounds of formula S1):
[0017]
[0018] Compared to compounds of formula S1), the compounds of formula I) according to the invention have an additional hydrogen donor in the form of a hydroxyl group, thus allowing the compounds of formula I) to scavenge more free radicals.
[0019] Combinations of different ageing stabilizer classes are also known from CN 105272892 and CN 107935867, for example combinations of phenols with aromatic amines. However, the individual units are not directly conjugated, but are always separated by aliphatic spacers. Therefore, there is no direct influence / interaction between these groups. Therefore, compared with the compounds from CN 105272892 and CN 107935867, the compounds of the invention with formula I) also have improved reactivity and thus improved protective action.
[0020] US 6770785 B1 discloses compounds having formulae S2 and S3.
[0021]
[0022] Compared with the compound of formula S2), the compound of formula I) of the present invention has the advantage that its units are conjugated, thus resulting in better protection. In formula S2), the conjugation is interrupted by the -CH2-NH moiety.
[0023]
[0024] Compared with compounds of formula S3), the compounds of the invention of formula I) have the advantage that the external nitrogen atom carries an aliphatic group instead of an aromatic group, thus resulting in better protection against ozone.
[0025] Compounds / molecules which have aliphatic or aromatic groups instead of 1,3-dimethylbutyl and hydrogen atoms only on the outer nitrogen atoms (i.e. without hydrogen atoms) and are therefore maximally substituted on the nitrogen atom likewise exhibit poorer protection against ozone than the compounds according to the invention according to formula I), since this part of the molecule has a decisive influence on the reactivity and the possibility of eliminating a hydrogen atom from the nitrogen atom jointly determines the protective effect.
[0026] The compounds of the formula I) according to the invention are particularly suitable as aging stabilizers and / or antiozonants in vehicle tires and / or in industrial rubber articles and / or in oils and / or lubricants, such as, in particular, air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber belts, profiles, seals, membranes, tactile sensors for medical or robotic applications, or shoe soles or parts thereof.
[0027] The compounds of the formula I) according to the invention are particularly suitable for producing rubber articles, in particular air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber belts, profiles, seals, membranes, tactile sensors for medical or robotic applications, or shoe soles or parts thereof.
[0028] To use the compound according to formula I) in the preparation or substance, the compound is employed in a composition and is used in conjunction with the composition.
[0029] In vehicle tires or other technical rubber products, this is in particular a rubber mixture.
[0030] The invention further provides the use of compounds of formula I) according to the invention in oils and lubricants, such as in particular fuels or fluids for engines. Thus, the compounds according to the invention can be used in engines.
[0031] The present invention further provides the use of the compounds according to the formula I) according to the invention as dyes in fibers and / or polymers and / or paper and / or in paints and coatings.
[0032] The invention therefore further provides a rubber mixture.
[0033] The rubber mixture according to the invention contains compounds of formula I). The rubber mixture according to the invention can in principle be any rubber mixture in which the novel compounds of formula I) achieve improved properties, in particular increased durability, by aging stability and / or anti-ozonation action.
[0034] The rubber mixture of the invention contains at least one rubber.
[0035] It is preferred when the rubber mixture according to the invention contains 0.1 to 10 phr, particularly preferably 0.1 to 5 phr, very particularly preferably 1 to 5 phr of a compound of the formula I).
[0036] The unit "phr" (parts per hundred parts of rubber by weight) used in this document is a conventional indication of the amount of a mixture formulation in the rubber industry. The dosages of parts by weight of the individual substances are in this document based on 100 parts by weight of the total mass of all high molecular weight (Mw greater than 20 000 g / mol) and therefore solid rubber present in the mixture.
[0037] In an advantageous embodiment of the invention, the rubber mixture according to the invention contains at least one diene rubber.
[0038] Thus, the rubber mixture may contain a diene rubber or a mixture of two or more different diene rubbers.
[0039] Diene rubber is a rubber formed by polymerization or copolymerization of a diene and / or a cycloolefin, and thus has a C═C double bond in the main chain or a side group.
[0040] The diene rubber is preferably selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, polyisoprene rubber having a molecular weight M greater than 20 000 g / mol ... w Liquid rubber, halogenated butyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile butadiene rubber and hydrogenated styrene-butadiene rubber.
[0041] In particular, nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halogenated butyl rubber and / or ethylene-propylene-diene rubber are used in the production of industrial rubber products such as belts, transmission belts and hoses, and / or shoe soles. Preferably, mixture compositions for these rubbers that are specific and known to those skilled in the art are used in terms of fillers, plasticizers, vulcanization systems and additives.
[0042] The natural polyisoprene and / or synthetic polyisoprene of all embodiments can be cis-1,4-polyisoprene or 3,4-polyisoprene. However, preference is given to using cis-1,4-polyisoprene with a cis-1,4 ratio of >90% by weight. Such polyisoprene can firstly be obtained by stereospecific polymerization in solution with a Ziegler-Natta catalyst or using finely dispersed alkyl lithium. Secondly, natural rubber (NR) is such a cis-1,4-polyisoprene, wherein the cis-1,4 content in the natural rubber is greater than 99% by weight.
[0043] Mixtures of one or more natural polyisoprenes with one or more synthetic polyisoprenes are furthermore conceivable.
[0044] In the context of the present invention, the term "natural rubber" is understood to mean the naturally occurring rubber that can be obtained from the Hevea rubber tree and "non-Hevea" sources. Non-Hevea sources include, for example, the Guayule shrub and dandelions such as, for example, TKS (Taraxacum rubber grass; Russian dandelion).
[0045] If the rubber mixture of the invention contains butadiene rubber (i.e. BR, polybutadiene), it can be of any type known to those skilled in the art. These include so-called high cis types and low cis types, polybutadiene having a cis content of not less than 90% by weight being referred to as high cis types, and polybutadiene having a cis content of less than 90% by weight being referred to as low cis types. An example of low cis polybutadiene is Li-BR (lithium catalyzed butadiene rubber) having a cis content of 20% to 50% by weight. Particularly good properties and low hysteresis of the rubber mixture are achieved with high cis BR.
[0046] The one or more polybutadienes used can be end-group modified and / or functionalized along the polymer chain by modification and functionalization. The modification can be selected from modifications with hydroxyl and / or ethoxy and / or epoxy and / or siloxane groups and / or amino and / or aminosiloxane and / or carboxyl and / or phthalocyanine groups and / or silane-sulfide groups. However, other modifications known to those skilled in the art, also referred to as functionalized, are also suitable. Metal atoms can be such functionalized components.
[0047] In the case where at least one styrene-butadiene rubber (styrene-butadiene copolymer) is present in the rubber mixture, it can be a solution-polymerized styrene-butadiene rubber (SSBR) or an emulsion-polymerized styrene-butadiene rubber (ESBR), and mixtures of at least one SSBR and at least one ESBR are also employable. The terms "styrene-butadiene rubber" and "styrene-butadiene copolymer" are used synonymously in the context of the present invention.
[0048] The styrene-butadiene copolymers used can be end-group modified and / or functionalized along the polymer chain by the modifications and functionalizations listed above for the polybutadienes.
[0049] The at least one diene rubber is preferably selected from the group consisting of natural polyisoprene (NR, natural rubber), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halogenated butyl rubber.
[0050] In a particularly preferred embodiment of the present invention, the at least one diene rubber is selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR) and emulsion polymerized styrene-butadiene rubber (ESBR).
[0051] In a particularly advantageous embodiment of the invention, the rubber mixture contains at least one natural polyisoprene (NR), preferably in an amount of 5 to 55 phr, and in a particularly advantageous embodiment of the invention, in an amount of 5 to 25 phr, very particularly preferably 5 to 20 phr. Such a rubber mixture exhibits good processing properties and reversion stability as well as optimal tearing properties and optimal rolling resistance characteristics.
[0052] In a particularly advantageous embodiment of the invention, the rubber mixture contains at least one polybutadiene (BR, butadiene rubber), preferably in an amount of 10 to 80 phr, particularly preferably 10 to 50 phr, and in a particularly advantageous embodiment of the invention, in an amount of 15 to 40 phr. This achieves particularly good tear and wear properties and optimal braking characteristics of the rubber mixture according to the invention.
[0053] In a particularly advantageous embodiment of the invention, the rubber mixture contains at least one solution polymerized styrene-butadiene rubber (SSBR), preferably in an amount of 10 to 80 phr, particularly preferably 30 to 80 phr, and in a particularly advantageous embodiment of the invention, in an amount of 50 to 70 phr. This achieves particularly good rolling resistance properties of the rubber mixture according to the invention. In a particularly advantageous embodiment of the invention, the SSBR is used in combination with at least one further rubber to achieve an optimal and balanced distribution of properties.
[0054] It is preferred that the rubber mixture contains at least one filler, preferably in an amount of 30 to 500 phr, particularly preferably 50 to 400 phr, further preferably 80 to 300 phr.
[0055] In an advantageous embodiment of the invention, the filler is a reinforcing filler preferably selected from the group consisting of carbon black and silica.
[0056] In a particularly advantageous embodiment of the invention, the rubber mixture contains at least one silicon dioxide as filler, preferably in an amount of 30 to 500 phr, particularly preferably 50 to 400 phr, and even more preferably 80 to 300 phr.
[0057] In these amounts, silica is especially present as the sole or main filler (greater than 50% by weight based on the total filler amount).
[0058] In a further advantageous embodiment of the invention, the rubber mixture contains at least one silicon dioxide as an additional filler, preferably in an amount of 5 to 100 phr, particularly preferably 5 to 80 phr, and even more preferably 10 to 60 phr.
[0059] In these amounts, silica is present in particular as a further filler in addition to another primary filler, such as in particular carbon black.
[0060] The silica may be any type of silica known to the person skilled in the art as being suitable as a filler for tire rubber mixtures. However, particular preference is given to using finely divided precipitated silica having a molecular weight of 35 to 400 m 2 / g, preferably 35 to 350m 2 / g, more preferably 85 to 320m 2 / g and most preferably 120 to 235m 2 / g nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132), and 30 to 400 m 2 / g, preferably 30 to 330m 2 / g, more preferably 80 to 300m 2 / g and most preferably 115 to 200 m 2 / g of CTAB surface area (according to ASTM D 3765). Such silica, for example, produces particularly good physical properties of the vulcanized product in rubber mixtures for tire treads. Advantages in the processing of the mixture by reducing the mixing time can also be produced here, while retaining the same product properties, which leads to improved productivity. The silica used can therefore be, for example, from Evonik Silica of the VN3 type (trade name) or highly dispersible silica known as HD silica (e.g. from Solvay) 1165MP).
[0061] In the case of the presence of at least two different silicas (which differ, for example, in their BET surface area) in the rubber mixture of the invention, the stated amount figures relate to the total amount of all silicas present.
[0062] The terms "silicic acid" and "silicon dioxide" are used synonymously in the context of the present invention.
[0063] The rubber mixture may additionally contain further fillers, such as in particular carbon black, in particular technical carbon black or pyrolytic carbon black, or further reinforcing or non-reinforcing fillers.
[0064] In the context of the present invention, further (non-reinforcing) fillers include aluminosilicates, kaolin, chalk, starch, magnesium oxide, titanium dioxide or rubber gel and also fibers (eg aramid fibers, glass fibers, carbon fibers, cellulose fibers).
[0065] Furthermore, optional reinforcing fillers are, for example, carbon nanotubes (CNTs), including discrete CNTs, hollow carbon fibers (HCFs) and modified CNTs containing one or more functional groups (such as hydroxyl, carboxyl and carbonyl groups), graphite and graphene, and so-called "carbon-silica dual-phase fillers".
[0066] In the context of the present invention, zinc oxide is not included among the fillers.
[0067] In a particularly advantageous embodiment of the invention, the rubber mixture according to the invention contains 0.1 to 60 phr, preferably 3 to 40 phr, particularly preferably 5 to 30 phr, very particularly preferably 5 to 15 phr of at least one carbon black. In these amounts, in addition to the main fillers, such as in particular silicon dioxide, carbon black is present in particular as an additional filler.
[0068] In a further advantageous embodiment of the present invention, the rubber mixture according to the present invention contains 30 to 300 phr, preferably 30 to 200 phr, particularly preferably 40 to 100 phr of at least one carbon black. In these amounts, the carbon black is present as the sole or main filler and is therefore optionally present in the above-mentioned lesser amount in combination with silica.
[0069] Suitable carbon blacks include any of the types of carbon blacks familiar to those skilled in the art.
[0070] In one embodiment, the carbon black has an iodine number (also referred to as iodine adsorption number) according to ASTM D 1510 of between 30 and 250 g / kg, preferably 30 to 180 g / kg, particularly preferably 40 to 180 g / kg and very particularly preferably 80 to 150 g / kg, and a DBP value according to ASTM D 2414 of 30 to 200 ml / 100 g, preferably 70 to 200 ml / 100 g, particularly preferably 90 to 200 ml / 100 g.
[0071] The DBP value according to ASTM D 2414 determines the specific absorption volume of carbon black or light-colored fillers by means of dibutyl phthalate.
[0072] The use of this type of carbon black in rubber mixtures, in particular for vehicle tires, ensures the best possible compromise between wear resistance and heat buildup, which in turn influences the ecologically relevant rolling resistance. It is preferred to use only one type of carbon black in the respective rubber mixture, but it is also possible to mix different types of carbon black into the rubber mixture.
[0073] In a particularly advantageous embodiment of the invention, the rubber mixture contains 5 to 60 phr, particularly preferably 5 to 40 phr, of at least one carbon black, and 50 to 300 phr, preferably 80 to 200 phr, of at least one silica.
[0074] The rubber mixture may further contain conventional additives in conventional weight portions, which are preferably added in at least one primary mixing stage during the production of the mixture. These additives include
[0075] a) ageing stabilizers known from the prior art, for example diamines, such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), or dihydroquinolines, such as 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ),
[0076] b) activators, for example zinc oxide and fatty acids (for example stearic acid) and / or other activators, such as zinc complexes, for example zinc ethylhexanoate,
[0077] c) activators and / or agents for binding fillers, in particular carbon black or silicon dioxide, for example S-(3-aminopropyl)thiosulfate and / or its metal salts (binding of carbon black) and silane coupling agents (binding of silicon dioxide),
[0078] d) antiozonant wax,
[0079] e) resins, especially tackifying resins for tire interior parts,
[0080] f) plasticizing aids, such as 2,2'-dibenzamidodiphenyl disulfide (DBD), and
[0081] g) processing aids, such as in particular fatty acid esters and metal soaps, for example zinc soaps and / or calcium soaps,
[0082] h) Plasticizers, such as, in particular, aromatic, naphthenic or paraffinic mineral oil plasticizers, for example MES (mild extraction solvate) or RAE (residual aromatic extract) or TDAE (treated distillate aromatic extract), or rubber liquid oils (RTL) or biomass liquid oils (BTL) preferably having a polycyclic aromatic hydrocarbon content of less than 3% by weight according to method IP 346, or triglycerides, for example rapeseed oil or oil paste or hydrocarbon resins or liquid polymers having an average molecular weight (determined by GPC=gel permeation chromatography according to BS ISO 11344:2004) of between 500 and 20 000 g / mol.
[0083] When a mineral oil is used, it is preferably selected from the group consisting of DAE (Distillate Aromatic Extract) and / or RAE (Residual Aromatic Extract) and / or TDAE (Treatened Distillate Aromatic Extract) and / or MES (Mild Extracted Solvent) and / or naphthenic oil.
[0084] In a particularly advantageous embodiment, the rubber mixture according to the invention contains no further aging stabilizers from the group of p-phenylenediamines (see above list a)) in addition to the compound of formula I). In a particularly preferred embodiment, the rubber mixture according to the invention contains in particular 0 to 0.1 phr, in particular 0 phr, of further aging stabilizers based on diamines selected from the group comprising, particularly preferably consisting of, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD).
[0085] Very small amounts of preferably 0 to 0 phr, particularly preferably 0 phr, of the abovementioned diamines and the compounds of formula I) present according to the invention can achieve an improved protective effect. The compounds of formula I) according to the invention replace the listed phenylenediamines known from the prior art.
[0086] In a further advantageous embodiment of the invention, at least one further representative of the diamine aging stabilizer is present and the compounds according to the invention thus only partially replace the diamines known from the prior art. This also achieves the advantages according to the invention, but not to the optimal extent.
[0087] In an advantageous embodiment, in addition to the compounds of formula I) according to the invention, an aging stabilizer based on dihydroquinoline (such as TMQ) is present in the rubber mixture. The amount of dihydroquinoline (such as especially TMQ) present is preferably 0.1 to 3 phr, in particular 0.5 to 1.5 phr.
[0088] In a further advantageous embodiment, the rubber mixture according to the invention comprises no further aging stabilizers, ie 0 phr of further aging stabilizers other than the compound of the invention of formula I).
[0089] The silane coupling agent may be of any type known to those skilled in the art.
[0090] Furthermore, one or more different silane coupling agents can be used in combination with one another. The rubber mixture can therefore contain a mixture of different silanes.
[0091] Silane coupling agents react with surface silanol groups or other polar groups of silica during mixing of the rubber / rubber mixture (in situ) or in the context of pretreatment (premodification) even before adding fillers to the rubber.
[0092] Coupling agents known from the prior art are difunctional organosilanes which have at least one alkoxy, cycloalkoxy or phenoxy group as a leaving group on the silicon atom and a group as a further functional group which, possibly after cleavage, can enter into a chemical reaction with the double bonds of the polymer. The latter group may, for example, comprise the following chemical groups:
[0093] -SCN, -SH, -NH2 or -S x -(where x=2 to 8).
[0094] Thus, silane coupling agents that can be used include, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'-bis(triethoxysilylpropyl)polysulfides having 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide (TESPD) or else mixtures of sulfides having 1 to 8 sulfur atoms with various sulfides in different contents. TESPT can also, for example, be used as a carbon black (trade name TESPD from Evonik) as a coupling agent. ) was added to the mixture.
[0095] End-capped mercaptosilanes, as are known, for example, from WO 99 / 09036, can also be used as silane coupling agents. It is also possible to use silanes as described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1 and WO 2008 / 083244 A1. It is also possible to use, for example, the silanes sold in various variants under the name NXT by Momentive, USA, or under the name VP Si The following are those sold by Evonik Industries.
[0096] The total proportion of further additives is preferably from 3 to 150 phr, more preferably from 3 to 100 phr and most preferably from 5 to 80 phr.
[0097] Zinc oxide (ZnO) may be included in the above-mentioned amount in the total ratio of the other additives.
[0098] This can be any type of zinc oxide known to those skilled in the art, such as ZnO granules or powder. Conventionally used zinc oxide usually has a particle size of less than 10 m 2 However, it is also possible to use a BET surface area of 10 to 100 m 2 / g of BET surface area of zinc oxide, such as the so-called "nano zinc oxide".
[0099] The rubber mixtures according to the invention are preferably used in vulcanized form, in particular in vehicle tires or other vulcanized industrial rubber articles.
[0100] The vulcanization of the rubber mixture of the present invention is preferably carried out in the presence of sulphur and / or sulphur donors with the aid of vulcanization accelerators, some of which may simultaneously act as sulphur donors. The accelerator is selected from the group consisting of thiazole accelerators and / or thiol-containing accelerators and / or sulfenamide accelerators and / or thiocarbamate accelerators and / or thiuram accelerators and / or thiophosphate accelerators and / or thiourea accelerators and / or xanthate accelerators and / or guanidine accelerators.
[0101] It is preferred to use a sulfonamide accelerator selected from the group consisting of N-cyclohexyl-2-benzothiazolesulfenamide (CBS) and / or N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or benzothiazolyl-2-sulfenomorpholide (MBS) and / or N-tert-butyl-2-benzothiazolylsulfenamide (TBBS) or a guanidine accelerator such as diphenylguanidine (DPG).
[0102] The sulfur-donating substance used may be any sulfur-donating substance known to the person skilled in the art. If the rubber mixture contains a sulfur-donating substance, the latter is preferably selected from the group comprising, for example, thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD) and / or tetramethylthiuram disulfide (TMTD) and / or tetraethylthiuram disulfide (TETD), and / or thiuram tetrasulfides, such as dipentamethylenethiuram tetrasulfide (DPTT), and / or dithiophosphates, such as DipDis (bis(diisopropyl)phosphorothioyl disulfide) and / or bis(O,O-2-ethylhexylphosphorothioyl)polysulfide (e.g. Rhenocure SDT Rheinchemie GmbH) and / or zinc dichlorooxydithiophosphate (e.g. Rhenocure Rhein Chemie) and / or zinc alkyl dithiophosphates and / or 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane and / or diaryl polysulfides and / or dialkyl polysulfides.
[0103] Other network-forming systems, such as those available for example under the trade name or A network-forming system obtained under the conditions of WO 2010 / 049216 A2 or a network-forming system as described in WO 2010 / 049216 A2 can also be used in the rubber mixture. Such a system contains a vulcanizing agent crosslinking with a functionality greater than four and at least one vulcanization accelerator.
[0104] Particular preference is given to using the accelerators TBBS and / or CBS and / or diphenylguanidine (DPG).
[0105] Vulcanization retarders may also be present in the rubber mixture.
[0106] The terms "vulcanized" and "cross-linked" are used synonymously in the context of the present invention.
[0107] In a preferred development of the invention, accelerators are added in the final mixing stage during the production of the sulfur-crosslinkable rubber mixture.
[0108] Sulfur cross-linkable rubber mixture of the present invention is produced by the usual method in the rubber industry, wherein the basic mixture of all the ingredients except the vulcanization system (sulfur and the material that affects the vulcanization) is first produced in one or more mixing stages. The final mixture is produced by adding the vulcanization system in the last mixing stage. For example, the final mixture is further processed and made into a suitable shape by means of extrusion operation or calendering.
[0109] This is followed by further processing by vulcanization, wherein, due to the addition of a vulcanization system in the context of the present invention, sulfur crosslinking occurs.
[0110] The above-described rubber mixtures of the invention are particularly suitable for use in vehicle tires, in particular pneumatic vehicle tires.
[0111] For use in vehicle tires, the mixture as a final mixture before vulcanization is preferably brought into the shape of a tread and applied in a known manner during the production of a green vehicle tire.
[0112] As already described, the production of rubber mixture of the present invention is carried out, and this rubber mixture is used as the sidewall or other body mixture of vehicle tire.The difference is the shaping after the extrusion operation / calendering of the mixture.The shape of the rubber mixture not yet vulcanized for one or more different body mixtures thus obtained is then used for the construction of green tire.
[0113] Here, "body mixture" refers to the rubber mixture for the internal components of the tire, such as mainly rubber rollers, inner liner (inner layer), ring core profile, belt, tire shoulder, belt profile, carcass, bead reinforcement, bead profile, flange profile and hoop. The uncured green tire is subsequently vulcanized.
[0114] In order to use the rubber mixture of the invention in drive belts and other belts, in particular in conveyor belts, the extruded, not yet vulcanized mixture is brought into a suitable shape and is generally provided simultaneously or subsequently with strength members, such as synthetic fibers or steel cords. This generally provides a multilayer construction consisting of one and / or more layers of rubber mixture, one and / or more layers of identical and / or different strength members and one and / or more further layers of identical and / or another rubber mixture.
[0115] The invention further provides a vehicle tire which comprises, in at least one component, a rubber mixture according to the invention, which contains the compound according to the invention.
[0116] The vulcanized vehicle tire comprises at least one vulcanized rubber of rubber mixture according to the present invention in at least one component.Those skilled in the art know that most materials (for example rubber present) exist or can exist in the form of chemical change after mixing or only after vulcanization.
[0117] Within the context of the present invention, "vehicle tyres" are understood to mean vehicle pneumatic tyres and solid rubber tyres, including tyres for industrial and construction site vehicles, trucks, cars and two-wheeled vehicle tyres.
[0118] The vehicle tire according to the invention preferably comprises the rubber mixture according to the invention in at least one external component, wherein the external component is preferably the tread, the sidewall and / or the flange profile.
[0119] The vehicle tire according to the invention can therefore also comprise in two or more components a rubber mixture according to the invention with an optionally suitable composition, which contains the compound of the formula I) according to the invention.
[0120] The present invention further provides a process for preparing a compound of formula I), wherein the process comprises at least the following process steps:
[0121] a) providing a substance having the formula A)
[0122]
[0123] b) providing methyl isobutyl ketone (MIBK) and hydrogen or methyl isobutyl ketone (MIBK) and formic acid;
[0124] c) reacting the substance according to step a) with the substance according to step b), preferably in the presence of a hydrogenation catalyst, to obtain a substance having formula C)
[0125]
[0126] d) providing a Lewis acid, such as, in particular, boron tribromide (BBr3), aluminum trichloride (AlCl3), aluminum tribromide (AlBr3), boron trifluoride etherate (BF3*OEt2) or tin tetrachloride (SnCl4), or a Bronsted acid, such as, in particular, hydrogen iodide (HI) or hydrogen bromide (HBr);
[0127] e) reacting a substance of formula C) with the substance from step d) to obtain a substance of formula I)
[0128]
[0129] In step b), alternatively methyl isobutyl ketone (MIBK) and hydrogen are preferred over MIBK and formic acid.
[0130] It is preferred that the substance of formula C) present in step c) is dissolved in an organic solvent, preferably an aprotic solvent, such as especially dichloromethane (DCM) or chloroform (CHCl 3 ), and then reacted according to step e).
[0131] The present invention further provides a further process for preparing a compound of formula I), wherein the process comprises at least the following process steps:
[0132] a1) providing a substance having the formula A)
[0133]
[0134] b1) providing a Lewis acid, such as in particular boron tribromide (BBr3), aluminum trichloride (AlCl3), aluminum tribromide (AlBr3), boron trifluoride etherate (BF3*OEt2) or tin tetrachloride (SnCl4), or a Bronsted acid, such as in particular hydrogen iodide (HI) or hydrogen bromide (HBr);
[0135] c1) reacting the substance according to step a1) with the substance from step b1) to obtain a substance having formula C1)
[0136]
[0137] d1) providing methyl isobutyl ketone (MIBK) and hydrogen;
[0138] e1) reacting a substance of formula C1) with a substance from step d1), preferably in the presence of a hydrogenation catalyst, to obtain a substance of formula I)
[0139]
[0140] Preference is given to the process step in which the reaction with hydrogen is carried out using a suitable catalyst, which is referred to in the context of the present invention as a "hydrogenation catalyst".
[0141] The hydrogenation catalyst of the process (step c) / e1)) is preferably a noble metal catalyst, such as in particular palladium (Pd) or platinum (Pt). The noble metal is preferably employed on carbon (C), such as palladium on carbon (Pd / C).
[0142] Other known catalysts such as Raney nickel or copper chromite may also be used.
[0143] Preference is given to using palladium on carbon (Pd / C) as hydrogenation catalyst in step c).
[0144] Preference is given to using palladium on carbon (Pd / C) as hydrogenation catalyst in step e1).
[0145] The hydrogen pressure in the corresponding process steps using hydrogen is preferably from 1 to 40 bar, particularly preferably from 10 to 30 bar, very particularly preferably from 15 to 25 bar.
[0146] The hydrogenation reaction in step c) / e1) is preferably carried out in an autoclave, in particular in a stainless steel autoclave.
[0147] The temperature in process steps c) and e1) is preferably from room temperature (RT, in particular 20° C.) to 100° C., particularly preferably 40° C. to 80° C., very particularly preferably 40° C. to 70° C.
[0148] Too high a temperature leads to undesired hydrogenation of the aromatic components.
[0149] All process steps, in particular steps e) and c1), are advantageously carried out in a protective gas atmosphere.
[0150] Process steps e) and c1) are preferably carried out at a temperature of -78 (minus seventy eight)° C. to +20° C., particularly preferably -10° C. to +10° C., in particular 0° C.
[0151] The reaction in process step e) / c1) is in each case an ether cleavage. In principle, any substance which can carry out the desired ether cleavage of substance C) / A) is suitable. Substances used to carry out ether cleavage are also referred to as "ether cleavage reagents" in the context of the present invention.
[0152] Lewis acids such as, in particular, boron tribromide (BBr3), aluminum trichloride (AlCl3), aluminum tribromide (AlBr3), boron trifluoride etherate (BF3*OEt2) or tin tetrachloride (SnCl4) or Bronsted acids such as, in particular, hydrogen iodide (HI) or hydrogen bromide (HBr) can be used for this purpose, which Bronsted acids are familiar to the person skilled in the art and can be characterized by their pKa values.
[0153] Strong Bronsted acids have pKa values between -1.74 (minus one point seven four) and 4.5 (four point five), and very strong acids have pKa values less than -1.74, such as Online Lexikon (URL: https: / / roempp.thieme.de / lexicon / RD- 19-00110? searchterm=s%C3%A4ure disclosed in.
[0154] In the context of the present invention, very strong Brønsted acids with a pKa of less than -1.74 are preferred, such as in particular hydrogen iodide (HI) or hydrogen bromide (HBr).
[0155] In a particularly advantageous embodiment of the invention, c1) and e) employ Lewis acids, in particular boron tribromide (BBr3).
[0156] The substance of formula A) and boron tribromide (BBr3) and methyl isobutyl ketone (MIBK) are commercially available. The other said substitutes for BBr3 are also commercially available. BRIEF DESCRIPTION OF THE DRAWINGS
[0157] Figure 1a and Figure 1b The cleavage mechanism is shown. DETAILED DESCRIPTION
[0158] The present invention will be described in more detail below with reference to working examples.
[0159] The component having formula I) is prepared as follows:
[0160] X1): Synthesize N-(1,3-dimethylbutyl)-N'-p-methoxyphenyl-p-phenylenediamine (having formula C) according to step c) Compounds):
[0161]
[0162] 5.00 g (23.3 mmol, 1 equivalent) of 4-(4-methoxyphenylamino)aniline, 2.00 g of Pd / C (palladium on carbon C) (5%) (0.2 g on 4.67 mmol substrate) and 50.0 mL of methyl isobutyl ketone (MIBK) were weighed into a stainless steel autoclave equipped with a Teflon liner. The autoclave was then pressurized to 20 bar with hydrogen (H2) and stirred at 60°C for 10 hours. After the reaction was terminated, excess hydrogen was blown off and the suspension was passed through diatomaceous earth. Filter and wash with ethanol. Concentrate the filtrate to dryness and dry in vacuo. Purify the residue on silica gel (cyclohexane / acetate 100:0→80:20). Orange oil; yield 5.6 g (80% of theory).
[0163] 1 H-NMR (500MHz, DMSO-d6) δ=8.09(s,1H),6.94(td,J=7.6,1.5Hz,1H),6.88(dd,J=7.6,1.4Hz,1H ),6.69-6.63(m,2H),6.51(d,J=8.4Hz,1H),6.27(dd,J=8.5,2.5Hz,1H),6.21(d,J=2.5Hz,1H),4 .82(d,J=8.9Hz,1H),3.30(dt,J=8.6,6.5Hz,1H),1.70(dp,J=13.5,6.7Hz,1H),1.38(dt,J=13. 9,7.1Hz,1H),1.16(dt,J=13.5,6.8Hz,1H),1.02(d,J=6.1Hz,3H),0.87(dd,J=19.4,6.6Hz,6H).
[0164] 13 C-NMR (126 MHz, DMSO-d6) δ = 151.8, 143.0, 140.0, 133.0, 120.7, 116.0, 114.5, 113.6, 55.2, 46.1, 45.9, 26.3, 24.5, 22.8, 22.6, 20.87 (46.1 and 45.9 are separated due to enantiomers).
[0165] ESI-MS (electrospray ionization mass spectrometry) [M+H] + =299.
[0166] According to step e), N-(1,3-dimethylbutyl)-N'-p-hydroxyphenyl-p-phenylenediamine (the present invention has Synthesis of compounds of formula I):
[0167]
[0168] Under argon, 5.70 g (19.1 mmol, 1 eq) of N-(1,3-dimethylbutyl)-N'-p-methoxyphenyl-p-phenylenediamine was dissolved in 20.0 mL of anhydrous dichloromethane (DCM) and cooled to 0 ° C. 5.52 mL (57.3 mmol, 5 eq) of boron tribromide was dissolved in 15 mL of anhydrous DCM and added dropwise with caution. The mixture was stirred overnight and the reaction was terminated by adding a saturated NaHCO3 solution under protective gas and under ice cooling. 50 mL of a 3:1 mixture of acetic acid / isopropanol was added in addition. The organic phase was washed with a saturated NaHCO3 solution and a saturated NaCl solution and dried over MgSO4. Once the filtration was complete, the solvent was concentrated to dryness and dried in vacuo. Pale purple to blue solid; yield 4.8 g (88% of theoretical value).
[0169] 1 H-NMR (500MHz, DMSO-d6) δ = 8.63 (s, 1H), 6.95 (s, 1H), 6.76 (d, J = 8.7Hz, 2H), 6.71 (d,J=8.8Hz,2H),6.59(d,J=8.7Hz,2H),6.51-6.44(m,2H),4.71(d,J=8.2Hz,1H), 3.40-3.31(d,J=6.9Hz,1H),1.73(dp,J=13.4,6.7Hz,1H),1.49-1.37(m,1H),1.23 -1.15(m,1H),1.05(d,J=6.1Hz,3H),0.91(d,J=6.6Hz,3H),0.87(d,J=6.6Hz,3H).
[0170] 13 C-NMR (126 MHz, DMSO-d6) δ = 149.8, 142.5, 138.1, 133.9, 119.9, 117.0, 115.6, 113.3, 46.1, 45.9, 26.3, 24.5, 22.8, 22.6, 20.8 (46.1 and 45.9 are separated due to isomers).
[0171] ESI-MS [M+H] + =285.
[0172] In an alternative variant of the reaction according to step c), an intermediate compound of formula C) is prepared as follows:
[0173] X2): Synthesis of N-(1,3-dimethylbutyl)-N'-p-methoxyphenyl-p-phenylenediamine:
[0174]
[0175] Under protective gas, 0.40g palladium carbon (5%) is suspended in 20mL anhydrous ethanol, and 1.00g (4.67mmol, 1 equivalent) 4-(4-methoxyphenylamino) aniline, 0.88mL (23.3mmol, 5 equivalents) formic acid (23.3mmol, 5 equivalents) and 1.17mL (9.33mmol, 2 equivalents) methyl isobutyl ketone are added successively. The mixture is heated under reflux for 4 hours, the solid is filtered off, and the solvent is removed in vacuo. The residue is purified on silica gel (cyclohexane / acetate 100:0→80:20). Orange oil; yield is 1.0g (73% of theory).
[0176] The spectrum is identical to the first run (X1).
[0177] Performance of process step c) according to X1) is preferred due to better reproducibility and less by-product formation (formates as by-products from the reaction of amine and formic acid) compared to the process step according to X2).
[0178] The compounds of the present invention are also prepared by the following alternative synthetic routes:
[0179] According to step c1), N-p-hydroxyphenyl-p-phenylenediamine (compound having formula C1) is synthesized:
[0180]
[0181] Under protective gas, 20 mL of degassed acetic acid and 10 mL of hydrobromic acid were initially charged, and 1 g (4.67 mmol, 1 equivalent) of 4-(4-methoxyphenylamino)aniline was dissolved therein and stirred at 120° C. for 24 hours. Once the solution reached room temperature, it was neutralized with saturated NaHCO3 solution and extracted with a 3:1 acetate / isopropanol mixture. The solvent was removed and the residue was purified over silica gel (cyclohexane / acetate 1:1). Brown solid; yield 0.7 g (75% of theory).
[0182] 1 H-NMR (500MHz, DMSO-d6) δ = 8.64 (s, 1H), 6.94 (s, 1H), 6.73-6.68 (m, 4H), 6.59 (d, J = 8.8Hz, 2H), 6.48 (d, J = 8.6Hz, 2H), 4.56 (s, 2H).
[0183] According to step e1), (1,3-dimethylbutyl)-N'-p-hydroxyphenyl-p-phenylenediamine (the present invention has the formula I) of the compound):
[0184]
[0185] 0.31 g (1.55 mmol, 1 equivalent) of N-p-hydroxyphenyl-p-phenylenediamine, 0.66 g of palladium on carbon (5%) (0.2 g on 4.67 mmol of substrate) and 20.0 mL of methyl isobutyl ketone were weighed into a stainless steel autoclave lined with Teflon. The autoclave was then pressurized to 20 bar with hydrogen and stirred at 60° C. for 10 hours. After the reaction was terminated, excess hydrogen was blown off and the suspension was passed through diatomaceous earth. Filter and wash with ethanol. Concentrate the filtrate to dryness and dry in vacuo. According to NMR analysis, the crude product contains 70% of the target molecule.
[0186] The compounds of the present invention having formula I) exhibit an increased reactivity relative to 6PPD. This is for example related to the binding dissociation energy (BDE) and the free activation enthalpy Δ R G ≠ and the free standard reaction enthalpy Δ R G o These values are reported in Table 1. Figure 1a and Figure 1b The cracking mechanism is shown, with values related to:
[0187] Table 1
[0188] molecular BDE[kJ / mol] <![CDATA[Δ R G o [kJ / mol]]]> <![CDATA[Δ R G ≠ [kJ / mol]]]> 6PPD 313 -25.6 19.1 Formula I) 305 -28.8 16.0
[0189] It is clear from Table 1 that the compounds of the present invention having formula I) have lower bond dissociation energy and lower free enthalpy.
[0190] The compounds of the formula I) therefore make it possible to achieve an improved protective effect in the applications mentioned.
[0191] For use in rubber mixtures for vehicle tires, the compounds of the invention with formula I) are added in a mixing stage in the production of the rubber mixture in a manner known to the person skilled in the art, for example instead of the aging stabilizers known in the prior art, such as 6PPD, 7PPD or IPPD etc.
Claims
1. A compound having formula I): I) 2. A rubber mixture comprising the compound of formula I) as claimed in claim 1.
3. The rubber mixture according to claim 2, characterized in that The rubber mixture contains at least one diene rubber.
4. The rubber mixture according to claim 3, characterized in that The rubber mixture contains at least one diene rubber selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halogenated butyl rubber.
5. A vehicle tire comprising the rubber mixture as claimed in any one of claims 2 to 4 in at least one component.
6. The vehicle tire according to claim 5, characterized in that The vehicle tire contains at least one rubber mixture as claimed in any one of claims 2 to 4 in at least one outer component.
7. The vehicle tire according to claim 6, characterized in that The external component is a tread, sidewall and / or flange profile.
8. A method for preparing a compound of formula I) as claimed in claim 1, the method comprising: At least the following method steps: a) providing a substance having the formula A) A) b) providing methyl isobutyl ketone (MIBK) and hydrogen or methyl isobutyl ketone (MIBK) and formic acid; c) reacting the substance according to step a) with the substance according to step b) to obtain a substance having formula C) C) d) providing a Lewis acid or a Bronsted acid; e) reacting the substance of formula C) with the substance from step d) to obtain the substance of formula I) I) 9. The method according to claim 8, characterized in that The Lewis acid is boron tribromide (BBr3), aluminum trichloride (AlCl3), aluminum tribromide (AlBr3), boron trifluoride ether complex (BF3*OEt2) or tin tetrachloride (SnCl4).
10. The method according to claim 8, characterized in that The Bronsted acid is hydrogen iodide (HI) or hydrogen bromide (HBr).
11. A method for preparing a compound of formula I) as claimed in claim 1, the method comprising: At least the following method steps: a1) providing a substance having the formula A) A) b1) providing a Lewis acid or a Bronsted acid; c1) reacting the substance according to step a1) with the substance from step b1) to obtain a substance having formula C1) C1) d1) providing methyl isobutyl ketone (MIBK) and hydrogen; e1) reacting the substance of formula C1) with methyl isobutyl ketone (MIBK) from step d1) to obtain the substance of formula I) I) 12. The method according to claim 11, characterized in that The Lewis acid is boron tribromide (BBr3), aluminum trichloride (AlCl3), aluminum tribromide (AlBr3), boron trifluoride ether complex (BF3*OEt2) or tin tetrachloride (SnCl4).
13. The method according to claim 11, characterized in that The Bronsted acid is hydrogen iodide (HI) or hydrogen bromide (HBr).
14. Use of a compound of formula I) as claimed in claim 1 as an ageing stabilizer and / or antiozonant in vehicle tires and / or industrial rubber products and / or oils and / or lubricants.
15. The use according to claim 14, characterized in that These industrial rubber products are air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber belts, profiles, seals, membranes, tactile sensors for medical applications or robotic applications, or shoe soles or parts thereof.
16. Use of a compound of formula I) as claimed in claim 1 for producing rubber products.
17. The use according to claim 16, characterized in that The rubber article is an air spring, a bellows, a conveyor belt, a belt, a drive belt, a hose, a rubber belt, a profile, a seal, a membrane, a tactile sensor for medical applications or robotic applications, or a shoe sole or parts thereof.
18. Use of a compound of formula I) as claimed in claim 1 in oils and lubricants.
19. The use according to claim 18, characterized in that The use is use in fuel or fluid for engines.
20. Use of a compound of the formula I) as claimed in claim 1 as a dye in fibers and / or polymers and / or paper and / or in paints and coatings.
Citation Information
Patent Citations
Antiozonant cum antioxidant, process for preparation
US6770785B1
Blocked mercaptosilane coupling agents for filled rubbers
WO1999009036A1
Tire compositions and components containing free-flowing filler compositions
WO2008083241A2
Tire compositions and components containing silated cyclic core polysulfides
WO2008083242A1
Tire compositions and components containing free-flowing filler compositions
WO2008083243A1