Adsorbent and preparation method thereof and method for purifying ethylene and alpha-olefin copolymers using the same

By using adsorbents with pyridine cations and hydrophilic groups, electrostatic forces and hydrogen bonding are used to efficiently remove residual halogen ions in the copolymer of ethylene and α-olefins, solving the problem of poor halogen removal effect in the existing technology. Improved product quality and equipment durability.

CN116351400BActive Publication Date: 2024-10-18WANHUA CHEM GRP CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211562887.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-10-18
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

It is difficult to effectively remove residual halogen ions in copolymers of ethylene and α-olefins with existing technology, especially when using metallocene catalysts. The presence of halogen affects product quality and equipment durability, and existing methods are not suitable for high-viscosity polymer solutions. The removal effect is not ideal or it is corrosive to the equipment.

Method used

Provide an adsorbent whose structure contains pyridine cations and hydrophilic groups, which combine with halogen ions through electrostatic force and hydrogen bonding, and can form a homogeneous solution with water to easily and efficiently remove different types of halogens from polymer solutions. ions, and regenerate the adsorbent through layered water washing and heated desorption.

Benefits of technology

It achieves efficient removal of residual halogen ions from the polymer solution, improves the purity of the polymer and the long-term safety of the equipment, and the adsorbent can be reused.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116351400B_ABST
    Figure CN116351400B_ABST
Patent Text Reader

Abstract

The present invention discloses an adsorbent and a preparation method thereof, and a method for purifying ethylene and α-olefin copolymer (POE) by using the adsorbent. The structural formula of the adsorbent is: the adsorbent can form a homogeneous solution with water, and is uniformly mixed and contacted with the ethylene and α-olefin copolymer obtained by catalysis of a halogenated metallocene compound, and halogen ions are easily adsorbed through electrostatic force and hydrogen bonding, and purified ethylene and α-olefin copolymer is obtained after layered water washing. The aqueous phase is heated to desorb halogen, and a poor solvent is added to obtain the adsorbent again. The adsorption process is simple and fast, and the removal rate of residual halogen ions is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adsorbents, and in particular to an adsorbent for removing residual halogen from ethylene and alpha-olefin copolymers and application thereof. Background Art

[0002] Polyolefins are one of the largest, most widely used and fastest growing varieties in polymer materials. The copolymer of ethylene and α-olefin is an important polymer material with low melting point, low crystallinity, low density, good flexibility and processing performance. The rapid development of polyolefins is accompanied by the continuous progress of olefin polymerization catalysts. As a new and efficient metallocene catalyst, the copolymer of ethylene and α-olefin obtained by the restricted geometry catalyst for olefin polymerization has the characteristics of long branching and narrow relative molecular mass distribution. Among them, polyolefin elastomer (POE) is a random copolymer prepared by catalytic polymerization of ethylene and 1-butene, 1-hexene or 1-octene by metallocene catalyst. The introduction of comonomer reduces the orderliness of polyethylene chain segments and reduces their crystallinity, thus giving POE good elasticity and excellent transparency; at the same time, a certain crystalline polyethylene phase is preserved in the POE molecule, which can be used as a physical crosslinking point to bear the load, making it have excellent thermoplasticity and is widely used in pipes, automobiles, food packaging, photovoltaics and other fields.

[0003] Early copolymers of ethylene and α-olefins used Ziegler-Natta catalysts, and the polymer activity was very low until the metallocene catalyst was discovered. Metallocene catalysts have an ideal single active center, and the electronegativity and spatial environment of the active center can be changed by changing its coordination group, thereby controlling the polymer microstructure and macroscopic performance. Chinese patents CN109957057B, CN1200007C, CN104892812A and CN104023844A all involve the use of metallocene catalysts to catalyze the synthesis of ethylene and α-olefin copolymers. However, the ethylene and α-olefin polymers manufactured using metallocene catalysts have the following problems, namely, they contain a small amount of halogen components derived from the catalyst, the obtained polymer has poor color tone or low transparency in quality, and white spots are generated when forming films. The halogens in the metallocene catalysts include F, Cl and Br, which are the most commonly used halogens in the industry. The presence of trace amounts of them will directly affect the product quality, and achieving complete removal has become the main research direction. In particular, the rapid growth of POE materials in the photovoltaic field requires us to pay attention to the impact of halogens in the products. The presence of halogen ions will directly affect its power generation effect and produce electric spots on the surface, affecting its durability and performance. In addition, the presence of halogens will also cause corrosion to the long-term operation of production equipment. Therefore, finding an effective purification method to effectively remove the residual halogen ions in the polymer is a key link in the synthesis of high-performance polyolefin materials. In the use of metallocene catalytic systems, the system belongs to a homogeneous catalyst. Although the catalyst has high activity and is suitable for reactions, the catalyst components are evenly dissolved in the solution containing the generated polymer, so it is difficult to remove the residual metal in the catalyst.

[0004] Chinese patent CN106630253A discloses a method of adding inorganic salts, silicates, phosphates and lime to treat chloride ions and generate insoluble metal compounds, which are separated to achieve the purpose of removal. However, this method is not ideal for high-viscosity polymer solutions.

[0005] Chinese patent CN103549642A uses anion exchange resin, which also reintroduces new impurity ions during the adsorption of chloride ions, and has limited ability to remove halogen ions uniformly dispersed in the polymer solution, and cannot meet very low requirements.

[0006] Chinese patent CN114804275A, this method uses N,N-dimethylformamide, p-nitrophenol, and isooctyl alcohol as raw materials, fully mixes them, and then washes them with dilute sulfuric acid to prepare an extractant to extract and remove chloride ions. However, this method requires the addition of an acidic solvent, which is obviously corrosive to the equipment and is not conducive to long-term use. In addition, the introduction of other solvents increases the solvent recovery step. Summary of the invention

[0007] In view of the above problems existing in the prior art, the purpose of the present invention is to provide an adsorbent and a preparation method, and a method for purifying ethylene and α-olefin polymers. The adsorbent of the present invention can form a homogeneous solution with water, and the halogen ions are easily adsorbed through electrostatic force and hydrogen bonding. After layered water washing, different types of halogens can be easily and efficiently removed from the polymer solution to obtain purified ethylene and α-olefin copolymers. The aqueous phase is heated to desorb the halogen, and a poor solvent is added to obtain the adsorbent again. The adsorption process is simple and rapid, and the removal rate of residual halogen ions in the α-olefin copolymer is high.

[0008] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0009] The present invention provides an adsorbent, the structure of which is shown in Formula 1:

[0010]

[0011] In the formula, R1 is independently selected from an ether group, and the ether group structure is Wherein p is 1 to 5, preferably 2 to 3, q ​​is 1 to 10, preferably 4 to 6;

[0012] R2 is independently selected from one or more of alkyl, alkoxy, amino, hydroxyl, carboxyl, aldehyde, carbonyl and ester, preferably one or more of C1-C3 alkyl, C1-C3 alkoxy, amino, hydroxyl, carboxyl, aldehyde, carbonyl and C1-C3 ester, more preferably one or more of amino, hydroxyl and carboxyl;

[0013] The value of n is 2-10, preferably 3-6.

[0014] The present invention also provides a method for preparing the adsorbent represented by the above formula 1, comprising the following steps:

[0015] (1) mixing the compound of formula 2 with an acid, a reactant, and a solvent A, heating to reflux to carry out reaction A, then adding an alkali solution A to adjust the pH to 7 to 8, and then washing with water and drying to obtain a compound of formula 3;

[0016] (2) mixing the compound of formula 3 with alkali solution B, terminal hydroxy ether of formula 4, phase transfer agent, and solvent B, heating to reflux to carry out reaction B, and then washing with water and drying to obtain a compound of formula 5;

[0017] (3) mixing the compound of formula 5 with the aliphatic hydrocarbon of formula 6 whose terminal group is halogen-substituted and solvent C, heating to reflux to carry out reaction C, filtering, washing with alcohol, and drying to obtain the adsorbent of formula 1;

[0018] The structural formulas of the compounds of formulas 2 to 6 are as follows:

[0019] That is, 3,5-diamino-4-bromopyridine;

[0020] R2 is defined the same as R2 in Formula 1, that is, R2 is independently selected from one or more of alkyl, alkoxy, amino, hydroxyl, carboxyl, aldehyde, carbonyl and ester, preferably one or more of C1-C3 alkyl, C1-C3 alkoxy, amino, hydroxyl, carboxyl, aldehyde, carbonyl and C1-C3 ester, more preferably one or more of amino, hydroxyl and carboxyl;

[0021] p and q are defined the same as p and q in Formula 1, that is, p is 1 to 5, preferably 2 to 3, and q is 1 to 10, preferably 4 to 6. For example, the terminal hydroxyl ether of Formula 4 can be selected from tetraethylene glycol and pentaethylene glycol;

[0022] R1 and R2 are defined the same as R1 and R2 in Formula 1, that is, R1 is selected from an ether group, and the ether group structure is wherein p is 1 to 5, preferably 2 to 3, q ​​is 1 to 10, preferably 4 to 6; R2 is independently selected from one or more of alkyl, alkoxy, amino, hydroxyl, carboxyl, aldehyde, carbonyl and ester, preferably one or more of C1 to C3 alkyl, C1 to C3 alkoxy, amino, hydroxyl, carboxyl, aldehyde, carbonyl and C1 to C3 ester, more preferably one or more of amino, hydroxyl and carboxyl;

[0023] X is independently selected from one of F, Cl and Br, and the value of n is the same as that in Formula 1, that is, the value of n is 2 to 10, preferably 3 to 6. For example, the terminal halogen-substituted aliphatic hydrocarbon in Formula 6 can be selected from 1,3-dichloropropane and 1,4-dichlorobutane.

[0024] In step (1) of the present invention, the acid is selected from at least one of permanganic acid, hydrochloric acid, nitric acid, sulfuric acid, perchloric acid, hydrobromic acid, trifluoromethanesulfonic acid, hydroiodic acid, and trifluoroacetic acid, preferably at least one of hydrochloric acid and trifluoromethanesulfonic acid;

[0025] The molar ratio of the compound of formula 2 to the acid is 1:2 to 2.5, preferably 1:2 to 2.2.

[0026] In step (1) of the present invention, the reactant is selected from azide compounds, peroxides, and chloroformate compounds, preferably at least one of sodium azide, hydrogen peroxide, and tert-butyl chloroformate;

[0027] The molar ratio of the compound of formula 2 to the reactant is 1:2 to 2.2, preferably 1:2.

[0028] In step (1) of the present invention, the solvent A is selected from at least one of tetrahydrofuran, diethyl ether, methyl tert-butyl ether and ethyl tert-butyl ether, more preferably at least one of tetrahydrofuran and methyl tert-butyl ether;

[0029] The volume amount of the solvent A is 10-20 mL / g, preferably 10-12 mL / g, relative to the mass of the compound of formula 2;

[0030] In step (1) of the present invention, the reflux temperature of reaction A is 65 to 85° C., preferably 70 to 85° C., and the reaction time is 4 to 8 hours, preferably 6 to 8 hours.

[0031] In step (1) of the present invention, the alkali solution A is an aqueous solution of alkali, wherein the alkali is selected from at least one of alkali metal hydroxides, preferably at least one of sodium hydroxide and potassium hydroxide;

[0032] The concentration of the alkali solution A is 1-3 mol / L, preferably 1-2 mol / L.

[0033] In step (1) of the present invention, after the reaction A is completed, post-treatment processes such as water washing and drying are also included, which are conventional operations in the field and are not specifically limited in the present invention. For example, the method used in some specific examples is water washing and layering, taking the organic phase and adding anhydrous sodium sulfate to dry, and then spinning the solvent to dry.

[0034] In step (2) of the present invention, the alkali solution B is an aqueous solution of alkali, wherein the alkali is selected from at least one of alkali metal carbonates, bicarbonates, and alkoxides, preferably at least one of sodium bicarbonate, sodium carbonate, cesium carbonate, potassium carbonate, and sodium ethoxide, and more preferably potassium carbonate;

[0035] The concentration of the alkali solution B is 2-5 mol / L, preferably 3-4 mol / L;

[0036] The molar ratio of the compound of formula 3 to the alkali in the alkali solution B is 1:1 to 1.5, preferably 1:1 to 1.2.

[0037] In step (2) of the present invention, the molar ratio of the compound of formula 3 to the terminal hydroxy ether of formula 4 is 1:1 to 1.3, preferably 1:1 to 1.1.

[0038] In step (2) of the present invention, the phase conversion agent is selected from at least one of benzyltriethylammonium chloride (TEBA), tetrabutylammonium bromide (TBAB), tetrabutylammonium chloride, tetrabutylammonium hydrogen sulfate, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride, and tetradecyltrimethylammonium chloride, preferably tetrabutylammonium bromide;

[0039] The molar ratio of the compound of formula 3 to the phase conversion agent is 1:0.2-0.5, preferably 1:0.2-0.3.

[0040] In step (2) of the present invention, the solvent B is an aprotic solvent, selected from at least one of dimethyl sulfoxide, N,N-dimethylformamide, acetone, acetonitrile, and 1,3-dimethyl-2-imidazolidinone, preferably at least one of acetonitrile and N,N-dimethylformamide;

[0041] The volume amount of the solvent B is 10 to 50 mL / g, preferably 20 to 35 mL / g, relative to the mass of the compound of formula 3.

[0042] In step (2) of the present invention, the reflux temperature of reaction B is 85 to 120° C., preferably 85 to 100° C., and the reaction time is 6 to 12 h, preferably 8 to 10 h.

[0043] In step (2) of the present invention, after the reaction B is completed, post-treatment processes such as water washing and drying are also included, which are conventional operations in the field and are not specifically limited by the present invention. For example, the method used in some specific examples is water washing, drying the organic phase, and then spinning the solvent.

[0044] In step (3) of the present invention, the molar ratio of the compound of formula 5 to the terminal halogen-substituted aliphatic hydrocarbon of formula 6 is 1:0.3-0.5, preferably 1:0.45-0.5.

[0045] In step (3) of the present invention, the solvent C is an aprotic solvent, selected from at least one of dimethyl sulfoxide, N,N-dimethylformamide, acetone, acetonitrile, and tetrahydrofuran, preferably at least one of acetonitrile and tetrahydrofuran;

[0046] The volume amount of the solvent C is 5 to 50 mL / g, preferably 10 to 15 mL / g, relative to the mass of the compound of formula 5.

[0047] In step (3) of the present invention, the reflux temperature of reaction C is 85 to 100° C., preferably 90 to 95° C., and the reaction time is 6 to 10 h, preferably 8 to 10 h.

[0048] In step (3) of the present invention, after the reaction C is completed, post-treatment processes such as filtration, alcohol washing (preferably ethanol), and drying are also included, which are conventional operations in the field and are not specifically limited by the present invention. For example, in some specific examples, the method used is water washing, drying the organic phase, and then spinning the solvent.

[0049] The present invention also provides an application of the above-mentioned adsorbent, which is suitable for polymer purification in the field of polyolefins, and is particularly suitable for removing residual halogen ions in materials such as polyethylene, POP, and POE.

[0050] Preferably, the present invention provides a method for purifying ethylene and α-olefin copolymers, the method using the above-mentioned adsorbent, comprising the following steps:

[0051] 1) preparing the adsorbent into a homogeneous aqueous solution, then mixing it with the reaction solution of ethylene and α-olefin copolymer (POE), adsorbing it under stirring, and then standing to separate the layers to obtain an aqueous phase and an organic phase;

[0052] 2) The organic phase is subjected to alcohol precipitation, water washing and drying to obtain purified ethylene and α-olefin polymers.

[0053] In step 1) of the present invention, the concentration of the homogeneous aqueous solution of the adsorbent is 10 to 50 wt %, preferably 20 to 30 wt %, and most preferably the saturated solubility of the adsorbent;

[0054] The volume of the homogeneous aqueous solution is 0.2 to 0.5 times, preferably 0.4 to 0.5 times, the volume of the reaction solution of the ethylene and α-olefin copolymer.

[0055] In step 1) of the present invention, the ethylene and α-olefin copolymer (POE) reaction liquid is selected from the reaction liquid obtained by copolymerization of ethylene and α-olefin under the action of a halogenated metallocene catalyst. The copolymerization process is a method disclosed in the prior art, and the present invention does not specifically limit its specific preparation process. The technicians can prepare it by any feasible method based on the prior art according to the needs;

[0056] Wherein, the α-olefin is selected from at least one of 1-butene, 1-hexene and 1-octene;

[0057] Wherein, the halogenated metallocene catalyst is selected from a catalyst comprising a halogenated metallocene compound; the central metal of the metallocene compound is selected from Ti, Zr, and Hf; the halogenated element is selected from one of F, Cl, and Br;

[0058] The metallocene compound can be a compound of different central metals, such as Ti, Zr, Hf. Taking titanium metal as an example, it can be selected from 2,6-dimethylphenoxy (cyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (2-methylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (2,3-methylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (2,4-dimethylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (2 ,3,4-trimethylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (2,3,5-trimethylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (pentamethylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (2-tert-butylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (2,4-di-tert-butylcyclopentadiene) titanium dichloride, 2,6-dimethylphenoxy (indenyl) titanium dichloride, 2,6-dimethylphenoxy 2,4,6-trimethylphenoxy(cyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(2-methylcyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(2,3-methylcyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(2,4-dimethylcyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(2,3,4-trimethylcyclopentadiene)titanium dichloride, 2,4, 6-trimethylphenoxy(2,3,5-trimethylcyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(pentamethylcyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(2-tert-butylcyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(2,4-di-tert-butylcyclopentadiene)titanium dichloride, 2,4,6-trimethylphenoxy(indenyl)titanium dichloride, 2,4,6-trimethylphenoxy(fluorenyl)titanium dichloride, etc.

[0059] In step 1) of the present invention, the homogeneous aqueous solution can be directly added to the reaction solution after the polymerization reaction of ethylene and α-olefin is completed.

[0060] In step 1) of the present invention, the adsorption operation is carried out at a temperature of 50 to 90° C., preferably 70 to 80° C., and for a time of 1 to 15 minutes, preferably 5 to 10 minutes.

[0061] In step 1) of the present invention, the temperature of the static stratification operation is 50 to 90° C., preferably 70 to 80° C., and the time is 1 to 3 hours, preferably 1 to 1.5 hours.

[0062] In step 2) of the present invention, the alcohol precipitation, water washing and drying are conventional operations in the art and are not specifically limited in the present invention. For example, in some specific examples, the method adopted is to add ethanol for precipitation and filtration, add clean water for rinsing, and then place in a vacuum drying oven for drying to obtain purified ethylene and α-olefin polymers.

[0063] The adsorbent of the present invention can be recycled and regenerated by heating the water phase separated in step 1) for desorption, then adding a poor solvent to precipitate the adsorbent, and then filtering and drying to obtain the regenerated adsorbent.

[0064] In the method of the present invention, the heating desorption is carried out at a temperature of 20 to 50° C., preferably 30 to 40° C., and for a time of 1 to 5 hours, preferably 2 to 3 hours.

[0065] In the method of the present invention, the poor solvent is selected from at least one of methanol, ethanol, ethylene glycol, 1-propanol, 1,2-propylene glycol, 1,3-propylene glycol and glycerol, preferably at least one of 1,2-propylene glycol and 1,3-propylene glycol;

[0066] The amount of the poor solvent is 0.2 to 0.8 times the volume of the water phase, preferably 0.2 to 0.3 times.

[0067] In the adsorbent structure of the present invention, firstly, the pyridinium cation can provide electrostatic force and form a π bond with the anion due to its positive charge and the electron-deficient property of the pyridinium ring; at the same time, the 2-position of the pyridinium ring can provide a strong hydrogen bond to interact with the anion; in addition, the hydrophilic groups contained in the R1 and R2 groups, such as amino, carboxyl, hydroxyl, ether, etc., can increase its water solubility, form a homogeneous system, and are easier to mix, contact and separate; specifically, the adsorption mode of the adsorbent of the present invention for different halogens can be expressed as follows:

[0068]

[0069] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0070] The adsorbent provided by the present invention can simply and efficiently remove different types of halogens from a polymer solution, and has the advantages of fast adsorption rate, simple mixing method, and reusability. DETAILED DESCRIPTION

[0071] The following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the rights claimed by the present invention.

[0072] The sources of the main raw materials in the examples and comparative examples of the present invention are as follows. Other sources are obtained from common commercial channels unless otherwise specified:

[0073] 3,5-Diamino-4-bromopyridine was purchased from Shanghai Bid Pharmaceuticals, purity 98%

[0074] Trifluoromethanesulfonic acid was purchased from MacLean with a purity of 98%;

[0075] Concentrated hydrochloric acid was purchased from Aladdin, with a concentration of 12 mol / L;

[0076] Tetrahydrofuran was purchased from Inotech with a purity of 99%;

[0077] Sodium azide was purchased from Anaiji Chemical with a purity of 95%;

[0078] Hydrogen peroxide was purchased from MacLean with a purity of 99.5%;

[0079] Tert-butyl chloroformate was purchased from MacLean with a purity of 98%;

[0080] Sodium hydroxide was purchased from Maclean with a purity of 96%;

[0081] Potassium carbonate was purchased from Aladdin with a purity of 99%;

[0082] Tetraethylene glycol was purchased from Aladdin Chemical with a purity of 99%;

[0083] Pentaethylene glycol was purchased from Aladdin Chemical with a purity of 98%;

[0084] Tetrabutylammonium bromide was purchased from Aladdin Chemical with a purity of 99%;

[0085] Acetonitrile was purchased from Inotech with a purity of 98%;

[0086] 1,3-Propanediol was purchased from Inokai with a purity of 98%;

[0087] 1,3-Dichloropropane was purchased from MacLean with a purity of 98%;

[0088] 1,4-Dichlorobutane was purchased from MacLean with a purity of 98%;

[0089] Isoper E alkane solvent was purchased from ExxonMobil;

[0090] Ethylene was purchased from Tianjin Saimet Chemical Technology Co., Ltd.;

[0091] 1-Octene was purchased from Aladdin with a purity of 98%;

[0092] 1-Hexene was purchased from Aladdin with a purity of 98%.

[0093] The main analytical methods used in the examples and comparative examples of the present invention are:

[0094] About 10 grams of polymer is burned with oxygen to convert the fluorine and chlorine therein into hydrogen fluoride and hydrogen chloride. The hydrogen fluoride and hydrogen chloride are absorbed by water, and the generated hydrogen fluoride and hydrogen chloride solutions are measured by ion chromatography. According to the retention time of the measured fluorine and chloride ions on the analytical column, the corresponding peak height or peak area is obtained for quantitative analysis to obtain the fluorine and chlorine content (ppm) in the copolymer.

[0095] The final adsorbent was characterized by using 400 Hz H NMR spectroscopy.

[0096] Example 1

[0097] The steps for preparing adsorbent A are as follows:

[0098]

[0099] (1) 18.7 g (0.1 mol) of 3,5-diamino-4-bromopyridine was added to a 500 mL round-bottom flask, and 200 mL of tetrahydrofuran, 33 g (0.22 mol) of trifluoromethanesulfonic acid and 13 g (0.2 mol) of sodium azide were added, and the mixture was heated under reflux at 80° C. for 8 hours. After the reaction was completed, a 2 mol / L sodium hydroxide aqueous solution was added to adjust the pH to 7-8, the mixture was washed with water and separated into layers, anhydrous sodium sulfate was added to the organic phase and dried, and the solvent was spin-dried to obtain a compound of formula 3;

[0100] NMR characterization: H 1 NMR(400MHz, CDCl3)δ2.0(4H,s),4.0(2H,s),7.77(2H,s)

[0101] (2) 21.8 g (0.1 mol) of the compound of formula 3 was placed in a 500 mL round-bottom flask, and 25 mL of an aqueous solution containing 13.8 g (0.10 mol) of potassium carbonate, 21.2 g (0.11 mol) of tetraethylene glycol and 440 mL of acetonitrile solvent, and 6.4 g (0.02 mol) of tetrabutylammonium bromide were added. The mixture was heated under reflux at 85° C. for 10 hours. After the reaction was completed, the mixture was washed with water three times. After the organic phase was dried, the solvent was dried by spin drying to obtain a compound of formula 5.

[0102] NMR characterization: H 1 NMR(400MHz, CDCl3)δ2.0(4H,s),3.44(2H,m),3.54-3.56(11H,m),3.79(2H,dd),4.0(2H,s),4.31(2H,t),7.7(2H,s)

[0103] (3) Take 66.2 g (0.2 mol) of the compound of the above formula 5 in a 1 L round-bottom flask, add 11.3 g (0.1 mol) of 1,3-dichloropropane, add 680 mL of tetrahydrofuran solvent, heat and reflux at 90° C. for 8 hours. After the reaction is completed, filter, rinse three times with ethanol, and dry to obtain the adsorbent A shown in formula 1.

[0104] NMR characterization: H 1 NMR(400MHz, CDCl3)δ2.0(8H,dd),2.26(2H,m),3.44(4H,m),3.54-3.56(22H,m),3.79(4H,dd),4.0-4.04(8H,s),4.31(4H,t),8.19(4H,s)

[0105] Example 2

[0106] Prepare adsorbent B as follows:

[0107]

[0108] (1) 18.7 g (0.1 mol) of 3,5-diamino-4-bromopyridine was added to a 500 mL round-bottom flask, and 200 mL of tetrahydrofuran, 16.7 ml (0.2 mol) of 12 mol / L concentrated hydrochloric acid and 11.3 g (0.2 mol) of a 60 wt % aqueous hydrogen peroxide solution were added, and the mixture was heated under reflux at 85° C. for 8 hours. After the reaction was completed, a 2 mol / L aqueous potassium hydroxide solution was added to adjust the pH to 7-8, the mixture was washed with water and the layers were separated. Anhydrous sodium sulfate was added to the organic phase and the mixture was dried. The solvent was spin-dried to obtain a compound of formula 3;

[0109] NMR characterization: H 1 NMR(400MHz, CDCl3)δ1.8(2H,m),3.8(2H,s),7.56(2H,s)

[0110] (2) 21.7 g (0.1 mol) of the compound of formula 3 was placed in a 500 mL round-bottom flask, and 30 mL of an aqueous solution containing 12.7 g (0.12 mol) of sodium carbonate, 21.2 g (0.11 mol) of tetraethylene glycol and 440 mL of N,N-dimethylformamide solvent, and 5.5 g (0.02 mol) of tetrabutylammonium chloride were added. The mixture was heated under reflux at 100° C. for 8 hours. After the reaction was completed, the mixture was washed with water three times. After the organic phase was dried, the solvent was dried by spin drying to obtain a compound of formula 5.

[0111] NMR characterization: H 1NMR(400MHz, CDCl3)δ1.9(2H,s),3.41(2H,m),3.52-3.54(11H,m),3.79(2H,dd),4.98(2H,s),4.30(2H,t),7.64(2H,s)

[0112] (3) Take 66.1 g (0.2 mol) of the compound of the above formula 5 in a 1 L round-bottom flask, add 11.3 g (0.1 mol) of 1,3-dichloropropane, add 700 mL of acetonitrile solvent, heat reflux at 90° C. for 10 hours, and after the reaction is completed, filter, rinse three times with ethanol, and dry to obtain the adsorbent B shown in formula 1.

[0113] NMR characterization: H 1 NMR(400MHz, CDCl3)δ1.87(4H,dd),2.15(2H,m),3.41(4H,m),3.54-3.58(22H,m),3.78(4H,dd),4.0-4.1(8H,s),4.29(4H,t),8.14(4H,s)

[0114] Example 3

[0115] The steps for preparing adsorbent C are as follows:

[0116]

[0117] (1) 18.7 g (0.1 mol) of 3,5-diamino-4-bromopyridine was added to a 500 mL round-bottom flask, and 200 mL of methyl tert-butyl ether, 33 g (0.22 mol) of trifluoromethanesulfonic acid and 27.3 g (0.2 mol) of tert-butyl chloroformate were added, and the mixture was heated under reflux at 85° C. for 8 hours. After the reaction was completed, a 2 mol / L potassium hydroxide aqueous solution was added to adjust the pH to 7-8, the mixture was washed with water and separated into layers, anhydrous sodium sulfate was added to the organic phase and dried, and the solvent was spin-dried to obtain a compound of formula 3;

[0118] NMR characterization: H 1 NMR(400MHz, CDCl3)δ7.8(2H,m),9.2(2H,s),11.2(2H,s)

[0119] (2) 33.4 g (0.1 mol) of the compound of formula 3 was placed in a 1 L round-bottom flask, 30 mL of an aqueous solution containing 13.8 g (0.12 mol) of potassium carbonate, 21.2 g (0.11 mol) of tetraethylene glycol and 500 mL of acetone solvent, and 9.6 g (0.03 mol) of tetrabutylammonium bromide were added, and the mixture was heated under reflux at 100° C. for 8 hours. After the reaction was completed, the mixture was washed with water three times, the organic phase was dried, and the solvent was dried by spin drying to obtain a compound of formula 5;

[0120] NMR characterization: H 1 NMR(400MHz, CDCl3)δ3.46(2H,m),3.55-3.58(11H,m),3.81(2H,dd),4.34(2H,s),8.04(2H,s),9.15(2H,s),11.2(2H,s)

[0121] (3) Take 89.5 g (0.2 mol) of the compound of the above formula 5 in a 1 L round-bottom flask, add 11.3 g (0.1 mol) of 1,3-dichloropropane, add 700 mL of acetone solvent, heat reflux at 90° C. for 9 hours, and after the reaction is completed, filter, rinse three times with ethanol, and dry to obtain the adsorbent C shown in formula 1.

[0122] NMR characterization:

[0123] H 1 NMR(400MHz, CDCl3)δ2.26(2H,m),3.45(4H,m),3.54-3.65(22H,m),3.85(4H,dd),4.34(4H,s),8.19(4H,s),9.17(4H,s),11.2(4H,s)

[0124] Example 4

[0125] Adsorbent D was prepared by following the steps of Example 1, except that tetraethylene glycol in step (2) was replaced by an equimolar amount of pentaethylene glycol to obtain adsorbent D shown in Formula 1.

[0126]

[0127] NMR characterization: H 1 NMR(400MHz, CDCl3)δ2.0(8H,dd),2.26(2H,m),3.44(4H,m),3.54-3.56(30H,m),3.79(4H,dd),4.0-4.04(8H,s),4.31(4H,t),8.19(4H,s)

[0128] Example 5

[0129] Adsorbent E was prepared by following the steps of Example 1, except that the sodium azide in step (1) was replaced by an equal molar amount of hydrogen peroxide, and the tetraethylene glycol in step (2) was replaced by an equal molar amount of pentaethylene glycol, to obtain adsorbent E shown in Formula 1.

[0130]

[0131] NMR characterization: H 1 NMR(400MHz, CDCl3)δ1.87(4H,dd),2.15(2H,m),3.41(4H,m),3.54-3.58(30H,m),3.78(4H,dd),4.0-4.1(8H,s),4.29(4H,t),8.14(4H,s)

[0132] Example 6

[0133] Adsorbent F was prepared by following the steps of Example 1, except that the sodium azide in step (1) was replaced by an equal molar amount of tert-butyl chloroformate, and the tetraethylene glycol in step (2) was replaced by an equal molar amount of pentaethylene glycol to obtain adsorbent F shown in Formula 1.

[0134]

[0135] NMR characterization:

[0136] H 1 NMR(400MHz, CDCl3)δ2.26(2H,m),3.45(4H,m),3.54-3.65(30H,m),3.85(4H,dd),4.34(4H,s),8.19(4H,s),9.17(4H,s),11.2(4H,s)

[0137] Example 7

[0138] Adsorbent G was prepared by following the steps of Example 1, except that 1,3-dichloropropane in step (1) was replaced by an equal molar amount of 1,4-dichlorobutane to obtain adsorbent G shown in Formula 1.

[0139]

[0140] NMR characterization: H 1 NMR(400MHz, CDCl3)δ1.74(4H,dd),2.0(8H,d)3.44(4H,m),3.54-3.56(20H,m) ,3.65(2H,m),3.79(4H,dd),4.0(4H,s),4.04(4H,dd),4.31(4H,t),8.19(4H,s)

[0141] Example 8

[0142] Adsorbent H was prepared by referring to Example 1, except that the sodium azide in step (1) was replaced by an equal molar amount of hydrogen peroxide, and the 1,3-dichloropropane in step (3) was replaced by an equal molar amount of 1,4-dichlorobutane, to obtain adsorbent H shown in Formula 1.

[0143]

[0144] NMR characterization: H 1 NMR(400MHz, CDCl3)δ1.72(4H,dd),2.2(4H,d),3.46(4H,m),3.56-3.60(20 H,m),3.68(2H,m),3.84(4H,dd),4.1-4.18(8H,m),4.31(4H,t),8.19(4H,s)

[0145] Example 9

[0146] Adsorbent I was prepared by referring to Example 1, except that the sodium azide in step (1) was replaced by an equal molar amount of tert-butyl chloroformate, and the 1,3-dichloropropane in step (3) was replaced by an equal molar amount of 1,4-dichlorobutane to obtain adsorbent I shown in Formula 1.

[0147]

[0148] NMR characterization:

[0149] H 1 NMR(400MHz, CDCl3)δ1.76(4H,m),3.47(4H,m),3.54-3.65(22H,m),3.85( 4H,dd),4.12(4H,m),4.34(4H,s),8.16(4H,s),9.15(4H,s),110.85(4H,s)

[0150] Example 10

[0151] The method for purifying ethylene and α-olefin copolymers using the adsorbent A prepared in Example 1 above comprises the following steps:

[0152] 1) Preparation of ethylene and α-olefin copolymer (POE) reaction liquid: In an ethylene atmosphere, 580 mL of Isoper E and 220 mL of 1-octene solution were added to a 2 L reactor, 2 mL of modified methylaluminoxane (MMAO), 0.5 μmol of 2,6-dimethylphenoxy (cyclopentadiene) titanium dichloride, ethylene was introduced and the pressure was maintained at 3 MPa, and the reaction was carried out at 70° C. for 30 min. After the reaction was completed, the system was depressurized to obtain an ethylene and 1-octene copolymer reaction liquid; 20 ml of the polymer solution was taken out and slowly added to ethanol to precipitate the polymer, which was washed with water, filtered and dried, and a chloride ion quantitative analysis test was performed, and it was found that the chloride ion content was 78 ppm.

[0153] 2) Add 0.5 times the volume of a homogeneous aqueous solution of adsorbent A (concentration of 20 wt%) to the reactor of the above-mentioned residual polymer solution, stir and adsorb at 70°C for 5 minutes, let it cool, release the mixed solution, and then let it stand at 70°C for 1 hour to separate the aqueous phase and the organic phase.

[0154] 3) The obtained aqueous phase was heated to 35° C. and stirred for 2 h to complete the desorption process. 0.2 times the volume of the poor solvent 1,3-propylene glycol was added to gradually precipitate the adsorbent A. The adsorbent A was then filtered and dried to obtain the regenerated adsorbent A with a recovery rate of 98%.

[0155] 4) The obtained organic phase polymerization liquid was added into 1 volume of ethanol, the polymer was precipitated, filtered, rinsed with water three times, and dried in a vacuum oven at 50° C. overnight to obtain a white polymer.

[0156] The residual chloride ions in the polymer were quantitatively analyzed by ion chromatography and found to be 1.4 ppm.

[0157] Repeat the above steps to purify the copolymer of ethylene and 1-octene, and apply the regenerated adsorbent A. The results are shown in Table 1:

[0158] Table 1

[0159]

[0160]

[0161] Embodiment 11

[0162] The method for purifying ethylene and α-olefin copolymers using the adsorbent B prepared in Example 2 above comprises the following steps:

[0163] 1) Preparation of ethylene and α-olefin copolymer (POE) reaction liquid: In an ethylene atmosphere, 540 mL of Isoper E and 260 mL of 1-octene solution were added to a 2 L reactor, 2.5 mL of modified methylaluminoxane (MMAO), 0.5 μmol of 2,6-dimethylphenoxy (pentamethylcyclopentadiene) titanium dichloride, ethylene was introduced and the pressure was maintained at 3.2 MPa, and the reaction was carried out at 140° C. for 15 min. After the reaction was completed, the system was depressurized to obtain an ethylene and 1-octene copolymer reaction liquid; 20 ml of the polymer solution was taken out and slowly added to ethanol, the polymer was precipitated, filtered and dried, and a fluoride ion quantitative analysis test was performed, and it was found that the chloride ion content was 81 ppm.

[0164] 2) Add 0.5 times the volume of a saturated aqueous solution of adsorbent B (concentration of 20 wt%) into the reactor of the above-mentioned residual polymer solution, stir and adsorb at 80°C for 3 minutes, let it cool, release the mixed solution, and then let it stand at 80°C for 1 hour to separate the layers to obtain the aqueous phase and the organic phase.

[0165] 3) The obtained aqueous phase was heated to 35° C. and stirred for 2 h to complete the desorption process. 0.3 times the volume of 1,3-propylene glycol was added to gradually precipitate the adsorbent B. The adsorbent B was then filtered and dried to obtain the regenerated adsorbent B with a recovery rate of 95%.

[0166] 4) The obtained organic phase polymerization liquid was added into 1 volume of ethanol, the polymer was precipitated, filtered, rinsed with water three times, and dried in a vacuum oven at 50° C. overnight to obtain a white polymer.

[0167] The residual chloride ions in the polymer were quantitatively analyzed by ion chromatography and found to be 1.1 ppm.

[0168] Repeat the above steps to purify the copolymer of ethylene and 1-octene, and apply the regenerated adsorbent B. The results are shown in Table 2:

[0169] Table 2

[0170]

[0171] Example 12

[0172] The method for purifying ethylene and α-olefin copolymers using the adsorbent C prepared in Example 3 above comprises the following steps:

[0173] 1) Preparation of ethylene and α-olefin copolymer (POE) reaction liquid: under ethylene atmosphere, add 500 mL of Isoper E and 300 mL of 1-hexene solution to a 2 L reactor, add 2.5 mL of modified methylaluminoxane (MMAO), 0.5 μmol of 2,4,6-trimethylphenoxy (cyclopentadiene) titanium dichloride, introduce ethylene and keep the pressure at 3.2 MPa, react at 85° C. for 10 min, and after the reaction is completed, release the pressure of the system to obtain ethylene and 1-hexene copolymer reaction liquid; take out 20 ml of the polymer solution and slowly add it to ethanol to precipitate the polymer, filter and dry it, and perform a quantitative analysis test of chloride ions, and it is found that the chloride ion content is 86 ppm.

[0174] 2) Add 0.5 times the volume of a saturated aqueous solution of adsorbent C (concentration of 20 wt%) into the reactor of the above-mentioned residual polymer solution, stir and adsorb at 70°C for 5 minutes, let it cool, release the mixed solution, and then let it stand at 70°C for 1 hour to separate the aqueous phase and the organic phase.

[0175] 3) The obtained aqueous phase was heated to 35° C. and stirred for 2 h to complete the desorption process. 0.2 times the volume of the poor solvent 1,3-propylene glycol was added to gradually precipitate the adsorbent A. The adsorbent A was then filtered and dried to obtain the regenerated adsorbent A with a recovery rate of 92%.

[0176] 4) The obtained organic phase polymerization liquid was added into 1 volume of ethanol, the polymer was precipitated, filtered, rinsed with water three times, and dried in a vacuum oven at 50° C. overnight to obtain a white polymer.

[0177] The residual chloride ions in the polymer were quantitatively analyzed by ion chromatography and found to be 0.8 ppm.

[0178] Repeat the above steps to purify the copolymer of ethylene and 1-hexene, and apply the regenerated adsorbent B. The results are shown in Table 3:

[0179] Table 3

[0180]

[0181]

[0182] Examples 13-18

[0183] The adsorbent DI prepared in the above Examples 4-9 was used to purify ethylene and α-olefin copolymers. The steps were similar to those in Example 10, except that the chloride ion content in the reaction solution of ethylene and α-olefin copolymers was replaced, and adsorbent A was replaced with adsorbent DI in turn. The results are shown in Table 4.

[0184] Comparative Example 1

[0185] The ethylene and α-olefin copolymer was purified by referring to the method of Example 10, except that adsorbent A was replaced by the compound of formula 5 prepared in Example 1, and other operations and conditions remained unchanged. The results are shown in Table 4.

[0186] Comparative Example 2

[0187] The ethylene and α-olefin copolymer was purified by referring to the method of Example 11, except that adsorbent B was replaced by the compound of formula 5 prepared in Example 2, and other operations and conditions remained unchanged. The results are shown in Table 4.

[0188] Comparative Example 3

[0189] The ethylene and α-olefin copolymer was purified by referring to the method of Example 12, except that the adsorbent C was replaced by the compound of formula 5 prepared in Example 3, and the other operations and conditions remained unchanged. The results are shown in Table 4.

[0190] Comparative Example 4

[0191] The ethylene and α-olefin copolymer was purified by referring to the method of Example 10, except that adsorbent A was replaced by the compound of formula 3 prepared in Example 1, and other operations and conditions remained unchanged. The results are shown in Table 4.

[0192] Comparative Example 5

[0193] The ethylene and α-olefin copolymer was purified by referring to the method of Example 11, except that adsorbent B was replaced by the compound of formula 3 prepared in Example 2, and other operations and conditions remained unchanged. The results are shown in Table 4.

[0194] Comparative Example 6

[0195] The ethylene and α-olefin copolymer was purified by referring to the method of Example 12, except that the adsorbent C was replaced by the compound of formula 3 prepared in Example 3, and the other operations and conditions remained unchanged. The results are shown in Table 4.

[0196] Table 4

[0197]

[0198]

Claims

1. An adsorbent, the structure of which is shown in Formula 1: In the formula, R1 is independently selected from an ether group, and the ether group structure is Where p ranges from 1 to 5, and q ranges from 1 to 10; R2 is independently selected from one or more of an alkyl group, an alkoxy group, an amino group, a hydroxyl group, a carboxyl group, an aldehyde group, a carbonyl group and an ester group; The value of n ranges from 2 to 10.

2. The adsorbent according to claim 1, characterized in that The value of p is 2 to 3, and the value of q is 4 to 6.

3. The adsorbent according to claim 1, characterized in that R2 is independently selected from one or more of a C1-C3 alkyl group, a C1-C3 alkoxy group, an amino group, a hydroxyl group, a carboxyl group, an aldehyde group, a carbonyl group and a C1-C3 ester group.

4. The adsorbent according to claim 3, characterized in that R2 is independently selected from one or more of amino, hydroxyl and carboxyl.

5. The adsorbent according to claim 1, characterized in that The value of n is 3 to 6.

6. A method for preparing the adsorbent according to any one of claims 1 to 5, characterized in that: The steps include: (1) mixing the compound of formula 2 with an acid, a reactant, and a solvent A, heating to reflux to carry out reaction A, then adding an alkali solution A to adjust the pH to 7 to 8, and then washing with water and drying to obtain a compound of formula 3; (2) mixing the compound of formula 3 with alkali solution B, terminal hydroxy ether of formula 4, phase conversion agent, and solvent B, heating to reflux to carry out reaction B, and then washing with water and drying to obtain a compound of formula 5; (3) mixing the compound of formula 5 with the aliphatic hydrocarbon of formula 6 whose terminal group is halogen-substituted and solvent C, heating to reflux to carry out reaction C, filtering, washing with alcohol, and drying to obtain the adsorbent of formula 1; The structural formulas of the compounds of formulas 2 to 6 are as follows: R2 is defined the same as R2 in Formula 1; p and q are defined the same as p and q in formula 1; R1 and R2 are defined the same as R1 and R2 in Formula 1; X is independently selected from one of F, Cl, and Br, and the value of n is the same as in Formula 1; Wherein, the reactant in step (1) is selected from azide compounds, peroxides, and chloroformate compounds.

7. The preparation method according to claim 6, characterized in that: In step (1), the acid is selected from at least one of permanganic acid, hydrochloric acid, nitric acid, sulfuric acid, perchloric acid, hydrobromic acid, trifluoromethanesulfonic acid, hydroiodic acid, and trifluoroacetic acid; The molar ratio of the compound of formula 2 to the acid is 1:2 to 2.5; and / or In step (1), the reactant is selected from at least one of sodium azide, hydrogen peroxide and tert-butyl chloroformate; The molar ratio of the compound of formula 2 to the reactant is 1:2 to 2.2; and / or In step (1), the solvent A is selected from at least one of tetrahydrofuran, diethyl ether, methyl tert-butyl ether and ethyl tert-butyl ether; The volume amount of the solvent A is 10-20 mL / g relative to the mass of the compound of formula 2; and / or In step (1), the reflux temperature of reaction A is 65-85° C. and the reaction time is 4-8 h; and / or In step (1), the alkali solution A is an aqueous solution of alkali, wherein the alkali is selected from at least one of alkali metal hydroxides; The concentration of the alkali solution A is 1-3 mol / L.

8. The preparation method according to claim 7, characterized in that: The molar ratio of the compound of formula 2 to the acid is 1:2 to 2.

2.

9. The preparation method according to claim 7, characterized in that: The molar ratio of the compound of formula 2 to the reactant is 1:

2.

10. The preparation method according to claim 7, characterized in that: The volume amount of the solvent A relative to the mass of the compound of formula 2 is 10-12 mL / g.

11. The preparation method according to claim 7, characterized in that: In the reaction A, the reflux temperature is 70-85° C. and the reaction time is 6-8 h.

12. The preparation method according to claim 7, characterized in that: The alkali solution A is an aqueous solution of alkali, wherein the alkali is selected from at least one of sodium hydroxide and potassium hydroxide.

13. The preparation method according to claim 7, characterized in that: The concentration of the alkali solution A is 1-2 mol / L.

14. The preparation method according to claim 6, characterized in that: In step (2), the alkali solution B is an aqueous solution of alkali, wherein the alkali is selected from at least one of alkali metal carbonates, bicarbonates, and alkoxides; The concentration of the alkali solution B is 2-5 mol / L; The molar ratio of the compound of formula 3 to the alkali in the alkali solution B is 1:1 to 1.5; and / or In step (2), the molar ratio of the compound of formula 3 to the terminal hydroxy ether of formula 4 is 1:1 to 1.3; and / or In step (2), the phase conversion agent is selected from at least one of benzyltriethylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium chloride, tetrabutylammonium hydrogen sulfate, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride, and tetradecyltrimethylammonium chloride; The molar ratio of the compound of formula 3 to the phase conversion agent is 1:0.2-0.5; and / or In step (2), the solvent B is an aprotic solvent; The volume amount of the solvent B is 10 to 50 mL / g relative to the mass of the compound of formula 3; and / or In step (2), the reflux temperature of reaction B is 85-120° C., and the reaction time is 6-12 h.

15. The preparation method according to claim 14, characterized in that: The base is selected from at least one of sodium bicarbonate, sodium carbonate, cesium carbonate, potassium carbonate and sodium ethoxide.

16. The preparation method according to claim 14, characterized in that: The concentration of the alkali solution B is 3-4 mol / L.

17. The preparation method according to claim 14, characterized in that: The molar ratio of the compound of formula 3 to the alkali in the alkali solution B is 1:1 to 1.

2.

18. The preparation method according to claim 14, characterized in that: The molar ratio of the compound of formula 3 to the terminal hydroxy ether of formula 4 is 1:1 to 1.

1.

19. The preparation method according to claim 14, characterized in that: The molar ratio of the compound of formula 3 to the phase conversion agent is 1:0.2-0.

3.

20. The preparation method according to claim 14, characterized in that: The solvent B is selected from at least one of dimethyl sulfoxide, N,N-dimethylformamide, acetone, acetonitrile, and 1,3-dimethyl-2-imidazolidinone.

21. The preparation method according to claim 14, characterized in that: The volume amount of the solvent B is 20-35 mL / g relative to the mass of the compound of formula 3.

22. The preparation method according to claim 14, characterized in that: In the reaction B, the reflux temperature is 85-100° C. and the reaction time is 8-10 h.

23. The preparation method according to claim 6, characterized in that: In step (3), the molar ratio of the compound of formula 5 to the aliphatic hydrocarbon of formula 6 whose terminal group is halogen-substituted is 1:0.3-0.5; and / or In step (3), the solvent C is an aprotic solvent; The volume amount of the solvent C is 5 to 50 mL / g relative to the mass of the compound of formula 5; and / or In step (3), the reflux temperature of reaction C is 85-100° C. and the reaction time is 6-10 h.

24. The preparation method according to claim 23, characterized in that: The molar ratio of the compound of formula 5 to the aliphatic hydrocarbon with halogen substituted terminal groups of formula 6 is 1:0.45-0.

5.

25. The preparation method according to claim 23, characterized in that: The solvent C is selected from at least one of dimethyl sulfoxide, N,N-dimethylformamide, acetone, acetonitrile and tetrahydrofuran.

26. The preparation method according to claim 23, characterized in that: The volume amount of the solvent C relative to the mass of the compound of formula 5 is 10-15 mL / g.

27. The preparation method according to claim 23, characterized in that: In the reaction C, the reflux temperature is 90-95° C. and the reaction time is 8-10 h.

28. Use of the adsorbent according to any one of claims 1 to 5 or the adsorbent prepared by the preparation method according to any one of claims 6 to 27 in the field of purification of polyolefins.

29. The use according to claim 28, characterized in that Suitable for removing residual halogen ions in polyethylene, POP and POE.

30. A method for purifying ethylene and α-olefin copolymers, characterized in that: The method uses the adsorbent according to any one of claims 1 to 5 or the adsorbent prepared by the preparation method according to any one of claims 6 to 27, comprising the following steps: 1) preparing the adsorbent into a homogeneous aqueous solution, then mixing it with the reaction solution of ethylene and α-olefin copolymer, adsorbing it under stirring, and then standing it for stratification to separate into an aqueous phase and an organic phase; 2) The organic phase is subjected to alcohol precipitation, water washing and drying to obtain purified ethylene and α-olefin polymers.

31. The method according to claim 30, characterized in that In step 1), the concentration of the adsorbent in the homogeneous aqueous solution is 10 to 50 wt %; The volume of the homogeneous aqueous solution is 0.2 to 0.5 times the volume of the reaction solution of the ethylene and α-olefin copolymer; and / or In step 1), the ethylene and α-olefin copolymer reaction liquid is selected from the reaction liquid obtained by copolymerization of ethylene and α-olefin under the action of a halogenated metallocene catalyst; Wherein, the α-olefin is selected from at least one of 1-butene, 1-hexene and 1-octene; Wherein, the halogenated metallocene catalyst is selected from a catalyst comprising a halogenated metallocene compound; the central metal of the metallocene compound is selected from Ti, Zr, Hf; the halogenated element is selected from one of F, Cl and Br; and / or In step 1), the homogeneous aqueous solution can be directly added to the reaction solution after the polymerization reaction of ethylene and α-olefin is completed; and / or In step 1), the adsorption operation is performed at a temperature of 50 to 90° C. for a time of 1 to 15 min; and / or In step 1), the static stratification operation is performed at a temperature of 50 to 90° C. and a time of 1 to 3 hours.

32. The method according to claim 31, characterized in that The homogeneous aqueous solution of the adsorbent has a concentration of 20 to 30 wt%.

33. The method according to claim 32, characterized in that The homogeneous aqueous solution of the adsorbent is the saturated solubility of the adsorbent.

34. The method according to claim 31, characterized in that The volume of the homogeneous aqueous solution is 0.4 to 0.5 times the volume of the reaction solution of the ethylene and α-olefin copolymer.

35. The method according to claim 31, characterized in that The adsorption operation is performed at a temperature of 70 to 80° C. and a time of 5 to 10 minutes.

36. The method according to claim 31, characterized in that The static stratification operation is performed at a temperature of 70 to 80° C. and a time of 1 to 1.5 hours.

37. The method according to claim 30, characterized in that The method for recovering and regenerating the adsorbent is as follows: heating the water phase separated in step 1) to desorb, then adding a poor solvent to precipitate the adsorbent, and then filtering and drying to obtain a regenerated adsorbent.

38. The method according to claim 37, characterized in that The heating desorption has a temperature of 20 to 50° C. and a time of 1 to 5 hours; The poor solvent is selected from at least one of methanol, ethanol, ethylene glycol, 1-propanol, 1,2-propylene glycol, 1,3-propylene glycol and glycerol; The amount of the poor solvent is 0.2 to 0.8 times the volume of the water phase.

39. The method according to claim 38, characterized in that The heating desorption has a temperature of 30 to 40° C. and a time of 2 to 3 hours.

40. The method according to claim 38, characterized in that The amount of the poor solvent is 0.2 to 0.3 times the volume of the water phase.

Citation Information

Patent Citations

  • Method for removing chloride ions from paper-making reconstituted tobaccos

    CN103549642A

  • Multinuclear metallocene catalyst compound for olefin polymerisation and copolymerisation and method for making thereof

    CN104023844A

  • Polyolefin thermoplastic elastomers and preparation method thereof

    CN104892812A

  • Coking wastewater chloride ion removing pretreatment method

    CN106630253A

  • An activation and feeding method for metallocene catalysts used in the preparation of POE