A preparation method and application of Pt-K / ATO catalyst
By preparing the Pt-K/ATO catalyst, the problems of limited resources of noble metal catalysts and poor water resistance in high-temperature reactions are solved, and the effect of simplifying the preparation process and improving catalytic activity is achieved. The catalyst exhibits excellent catalytic performance at high temperatures.
Patent Information
- Application Number
- CN202310260431.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-17
AI Technical Summary
In practical applications, precious metal catalysts have limited resources and are costly, and have poor water resistance and stability in high-temperature reactions. The process of adding alkali metals in the prior art is complicated and the catalyst activity is insufficient.
Using a preparation method of Pt-K/ATO catalyst, the loading amount is prepared by mixing potassium nitrate with chloroplatinic acid solution and adding ATO for ultrasonic dissolution and drying, and then performing a reduction reaction under a reducing atmosphere and high-temperature calcination. A catalyst of 0.1-1 wt% K and 0.05-1 wt% Pt.
The preparation process is simplified, the activity and water resistance of the catalyst are improved, and the catalyst exhibits excellent catalytic properties at high temperatures, and can complete the catalytic conversion of benzene at 200°C, with a conversion rate of 100%.
Smart Images

Figure CN116351415B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new material preparation, and specifically relates to a preparation method of a Pt-K / ATO catalyst and application thereof. Background Art
[0002] Precious metals (such as Pt, Pd, Ag and Au) are widely used as commercial catalysts for the catalytic combustion of benzene due to their excellent low-temperature performance and good stability in practical applications. However, precious metal resources are limited and expensive, so they cannot be used on a large scale. In recent years, in order to improve the activity and utilization rate of precious metals, scholars have formed new catalysts by adding cheap additives to overcome the problems of the scarcity of precious metals and the high cost of commercial catalysts.
[0003] Alkali metals are one of the widely used inexpensive additives that can promote catalysts to show improved activity in various reactions, such as preferential CO oxidation (PROX), water-gas shift reaction, and low-temperature oxidation of formaldehyde. In addition, the choice of catalyst carriers can also affect the catalytic activity. However, the process of adding alkali metals to catalysts is still very complicated, and the water stability of the obtained catalysts in high-temperature reactions is still poor. Summary of the invention
[0004] The present invention aims to overcome the defects of the prior art and provide a method for preparing a Pt-K / ATO catalyst.
[0005] Another object of the present invention is to provide application of the Pt-K / ATO catalyst prepared by the above preparation method.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing a Pt-K / ATO catalyst comprises the following steps:
[0008] (1) Potassium nitrate and chloroplatinic acid solution are mixed, ultrasonically dissolved, and then ATO is added, stirred and dispersed evenly, followed by drying;
[0009] (2) placing the material obtained in step (1) in a reducing atmosphere for reduction reaction to obtain a Pt-K / ATO precursor;
[0010] (3) calcining the Pt-K / ATO precursor to obtain the Pt-K / ATO catalyst, wherein the K loading is 0.1-1 wt % and the Pt loading is 0.05-1 wt %.
[0011] In a preferred embodiment of the present invention, the Pt-K / ATO catalyst has a K loading of 0.3 wt% and a Pt loading of 1 wt%.
[0012] Further preferably, the ratio of potassium nitrate, chloroplatinic acid solution and ATO is 0.39 g:25.6 mL:5 g.
[0013] In a preferred embodiment of the present invention, the drying temperature is 30-60°C.
[0014] More preferably, the drying temperature is 60°C.
[0015] In a preferred embodiment of the present invention, the reducing atmosphere is 20-60% H2 / N2, the temperature of the reduction reaction is 200-400°C, and the time is 1-4h.
[0016] Further preferably, the reducing atmosphere is 30% H2 / N2, the temperature of the reduction reaction is 200°C, and the time is 1 hour.
[0017] In a preferred embodiment of the present invention, the calcination temperature is 600-1000° C. and the calcination time is 1-5 h.
[0018] More preferably, the calcination temperature is 800° C. and the calcination time is 2 h.
[0019] Application of the Pt-K / ATO catalyst prepared by the above preparation method in catalytic oxidation of benzene.
[0020] The beneficial effects of the present invention are:
[0021] 1. The preparation process of the present invention does not involve complicated reactions and operation steps and is easy to operate and repeat.
[0022] 2. In the present invention, the introduction of alkali metal K promotes more inactive small clusters of Pt to grow into active Pt nanoparticles, thereby increasing the density of metal particles and improving the catalytic reaction activity.
[0023] 3. The present invention adopts a high-temperature calcination method to synthesize the Pt-K / ATO catalyst, so that it can have good water resistance stability in high-temperature reactions.
[0024] 4. The Pt-K / ATO catalyst prepared by the present invention has excellent catalytic performance. After being calcined at 800°C, it can catalyze benzene at 200°C with a conversion rate of 100%. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 These are high-angle annular dark-field scanning transmission electron microscope images of the Pt-K / ATO catalyst prepared in Example 1 and the Pt / ATO catalyst prepared in Example 2 in Example 3 of the present invention.
[0026] Figure 2The X-ray powder diffraction patterns of the Pt-K / ATO catalyst prepared in Example 1 and the Pt / ATO catalyst prepared in Example 2 in Example 4 of the present invention are shown in FIG.
[0027] Figure 3 This is a performance diagram of the catalytic oxidation of benzene by the Pt-K / ATO catalyst prepared in Example 1 and the Pt / ATO catalyst prepared in Example 2 in Example 5 of the present invention.
[0028] Figure 4 This is a performance diagram of the catalytic oxidation of benzene in an atmosphere containing H2O=5 vol% at 200°C over the Pt-K / ATO catalyst prepared in Example 1 in Example 6 of the present invention. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.
[0030] Example 1
[0031] A method for preparing a Pt-K / ATO catalyst comprises the following steps:
[0032] (1) 0.39 g potassium nitrate was mixed with 25.6 mL chloroplatinic acid solution, and ultrasonically dissolved. Then 5 g ATO was added and stirred to disperse evenly, and then dried in an oven at 60° C.;
[0033] (2) The material obtained in step (1) was placed in a reducing atmosphere for reduction reaction to obtain a Pt-K / ATO precursor. The reducing atmosphere was 30% H2 / N2 (200 mL min- 1 ), the reduction reaction temperature is 200°C and the time is 1h;
[0034] (3) The Pt-K / ATO precursor is calcined at a temperature of 800° C. for 2 h to obtain the Pt-K / ATO catalyst, wherein the K loading is 0.3 wt % and the Pt loading is 1 wt %.
[0035] Example 2
[0036] The difference between this embodiment and embodiment 1 is that 0.39 g of potassium nitrate is not added to obtain a Pt / ATO catalyst.
[0037] Example 3
[0038] The Pt-K / ATO catalyst prepared in Example 1 and the Pt / ATO catalyst prepared in Example 2 were used to prepare powder samples using a copper mesh. Deionized water was selected as a dispersant and ultrasonic treatment was performed. After drying, the samples were subjected to high-angle annular dark field imaging operation to observe the morphological images of the catalysts under dark field.
[0039] like Figure 1 As shown, compared with the Pt / ATO catalyst prepared in Example 2, the particle size of the Pt-K / ATO catalyst prepared in Example 1 does not change significantly, but the density of the metal particles can be seen to be increased from the density of the Pt nanoparticles in the figure.
[0040] Example 4
[0041] In order to analyze the crystal structure of the prepared catalyst, the Pt-K / ATO catalyst prepared in Example 1 and the Pt / ATO catalyst prepared in Example 2 were subjected to X-ray powder diffraction analysis.
[0042] like Figure 2 As shown in the figure, after the alkali metal K modified Pt / ATO, it can be clearly seen that the intensity of the Pt diffraction peak increased significantly. The results of comparing the half-peak width indicate that the size has not grown much, but the intensity of the Pt diffraction peak has increased. Combined with the experimental results of high-angle annular dark field imaging, it is speculated that more inactive small clusters of Pt grew into active Pt nanoparticles under the action of alkali metals, thus increasing the density of metal particles.
[0043] Example 5
[0044] The experimental steps of catalytic oxidation of benzene are as follows: Pt-K / ATO catalyst prepared in Example 1 and Pt / ATO catalyst prepared in Example 2 are pressed into tablets respectively and passed through a 40-60 mesh sieve, and 0.1 g of each is taken into a quartz tube with an inner diameter of 0.6 mm. A mixed gas of 500 ppm, 20 vol% O2 and balance gas N2 is introduced at a flow rate of 100 mL min-1. 1 The reactor temperature was raised to 130°C and the gas after the reaction was sent to the gas chromatograph to analyze the catalytic performance of the catalyst. Figure 3 .
[0045] from Figure 3 It can be seen that compared with the Pt / ATO catalyst without adding alkali metal, the Pt-K / ATO catalyst modified with alkali metal has better catalytic oxidation performance of benzene. After high-temperature calcination at 800°C, it can complete the catalysis of benzene at 200°C, and the conversion rate reaches 100%.
[0046] Example 6
[0047] The difference between this embodiment and embodiment 5 is that 5 vol% H2O is added to the mixed gas, the reactor is programmed to be heated to 130°C, and the gas after the reaction is sent to the gas chromatograph to analyze the catalytic performance of the catalyst. The water performance of the catalyst is shown in the figure Figure 4 .
[0048] from Figure 4It can be seen that the introduction of H2O has almost no effect on the catalytic activity of the sample. Therefore, the Pt-K / ATO catalyst prepared in Example 1 has good resistance to water vapor.
[0049] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. Application of Pt-K / ATO catalyst in catalytic oxidation of benzene, characterized in that: The preparation method of the Pt-K / ATO catalyst comprises the following steps: (1) Potassium nitrate and chloroplatinic acid solution were mixed, ultrasonically dissolved, and then ATO was added and stirred to disperse evenly, followed by drying at 60° C. The ratio of potassium nitrate, chloroplatinic acid solution and ATO was 0.39 g: 25.6 mL: 5 g; (2) placing the material obtained in step (1) in a reducing atmosphere of 30% H2 / N2 and subjecting it to a reduction reaction at 200°C for 1 hour to obtain a Pt-K / ATO precursor; (3) The Pt-K / ATO precursor was calcined at 800° C. for 2 h to obtain the Pt-K / ATO catalyst, wherein the K loading was 0.3 wt % and the Pt loading was 1 wt %.