Ferrite material, preparation method, near field communication antenna and communication equipment

By adjusting the composition ratio and process flow of ferrite materials, ferrite materials with moderate permeability were prepared, which solved the problem of discomfort in existing materials in near-field communication antennas, met the performance requirements and reduced the cost.

CN116354712BActive Publication Date: 2024-11-08DONGGUAN DEMEN ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310334108.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-11-08
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The actual magnetic permeability part of the existing ferrite material at a frequency of 13.56MHz cannot reach 180 or the imaginary part exceeds 5, resulting in excessive loss and cannot meet the performance requirements of near-field communication antennas.

Method used

The composition ratios of Fe2O3 60-70%, ZnO 15-22%, CuO 7-10%, NiO 7-9%, Co2O3 0.6-1.0%, LiF 0.2-0.4%, were adopted to pass ball milling, sieving, pre-firing and finalization. The firing process produces ferrite material with uniform grains and dense structures to ensure that the imaginary part of the magnetic permeability is less than 5 and the real part is greater than 235.

Benefits of technology

The imaginary magnetic permeability part of the ferrite material is less than 5 at 13.56MHz and the real magnetic permeability part is greater than 235, which meets the performance requirements of near-field communication antennas, and at the same time reduces the NiO content and reduces the material cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116354712B_ABST
    Figure CN116354712B_ABST
Patent Text Reader

Abstract

The present application discloses a ferrite material, a preparation method, a near field communication antenna and a communication device. The preparation method of the ferrite material comprises: ball milling a main component and an additive to obtain a slurry, wherein the main component comprises, by weight percentage: Fe 2 O 3 60-70%, ZnO 15-22%, CuO 7-10%, NiO 7-9%; based on the weight of the main component as 1, the additives include: Co 2 O 3 0.6-1.0%, LiF0.2-0.4%; sieving and pre-calcining the slurry to obtain a precursor powder; pressing the precursor powder into a shape, and finally calcining to obtain a ferrite material. The imaginary part of the magnetic permeability of the ferrite material prepared in the present application does not exceed 5 at 13.56MHz, and the real part of the magnetic permeability is greater than 235. In addition, the NiO content in the ferrite material of the present application is low, thereby reducing the cost of the ferrite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of ferrite materials, and in particular to a ferrite material, a preparation method, a near-field communication antenna and a communication device. Background Art

[0002] As electronic products develop towards smaller, thinner and lighter, the market has put forward higher requirements for magnetic sheets used for Near Field Communication (NFC) antennas, requiring that the real part of the magnetic permeability (u') of the magnetic sheet after fragmentation (including air gap) at a frequency of 13.56MHz should be no less than 180, and the imaginary part of the magnetic permeability (u") should be less than 5. This requires that the real part of the magnetic permeability before the magnetic sheet is fragmented should be above 200, or even greater than 235, and the imaginary part of the magnetic permeability should be less than 5.

[0003] The magnetic sheets made of existing ferrite materials either have a real part of magnetic permeability that cannot meet the requirements, or an imaginary part of magnetic permeability that exceeds 5, resulting in excessive losses. Summary of the invention

[0004] In response to the above technical problems, the present application provides a ferrite material, a preparation method, a near-field communication antenna and a communication device, which can improve the problem that the real part of the magnetic permeability of magnetic sheets made of current ferrite materials cannot meet the requirements or the imaginary part of the magnetic permeability exceeds 5, resulting in excessive losses.

[0005] In order to solve the above technical problems, in a first aspect, an embodiment of the present application provides a method for preparing a ferrite material, comprising:

[0006] The main component and the additive are ball-milled to obtain a slurry, wherein the main component comprises, by weight percentage, 60-70% of Fe2O3, 15-22% of ZnO, 7-10% of CuO, and 7-9% of NiO; based on the weight of the main component being 1, the additive comprises, 0.6-1.0% of Co2O3, and 0.2-0.4% of LiF;

[0007] The slurry is sieved and pre-calcined to obtain a precursor powder;

[0008] The precursor powder is pressed into a shape and then final fired to obtain the ferrite material.

[0009] Optionally, in the pre-firing step, the pre-firing temperature is 785-815° C. and the insulation time is 100-150 min.

[0010] Optionally, in the final firing step, the final firing temperature is 945-965° C. and the insulation time is 100-150 minutes.

[0011] Optionally, in the ball milling step, the weight ratio of the total weight of the main component and the additive to the grinding body and water is 1:1:1.

[0012] Optionally, the screening process includes:

[0013] The slurry is dried and then sieved through a 40-mesh screen.

[0014] Optionally, the pressing and molding of the precursor powder comprises:

[0015] The precursor powder is placed in a mold and then 2 The pressure is pressed into shape.

[0016] In a second aspect, an embodiment of the present application further provides a ferrite material, including a main component and an additive;

[0017] The main components include, by weight percentage, 60-70% Fe2O3, 15-22% ZnO, 7-10% CuO, and 7-9% NiO;

[0018] Based on the weight of the main component being 1, the additives include: Co2O3 0.6-1.0%, LiF 0.2-0.4%.

[0019] Optionally, the main components, measured by weight percentage, include: Fe2O3 63%, ZnO 20%, CuO 9%, and NiO 8%.

[0020] In a third aspect, an embodiment of the present application further provides a near field communication antenna, comprising a magnetic sheet, wherein the magnetic sheet comprises the ferrite material as described in the above embodiments, or is prepared by the preparation method as described in the above embodiments.

[0021] In a fourth aspect, an embodiment of the present application further provides a communication device, comprising the near field communication antenna as described in the above embodiments.

[0022] As described above, the present embodiment provides a method for preparing a ferrite material, wherein the ferrite material includes a main component and an additive, wherein the main component includes, by weight percentage, 60-70% Fe2O3, 15-22% ZnO, 7-10% CuO, and 7-9% NiO; taking the weight of the main component as 1, the additive includes 0.6-1.0% Co2O3 and 0.2-0.4% LiF. In the present embodiment, the main component and the additive are first ball-milled to obtain a slurry, and then the slurry is sieved and pre-fired to obtain a precursor powder; finally, the precursor powder is pressed into shape and finally fired to obtain a ferrite material. The ferrite material obtained in the present embodiment has uniform grains and a dense structure, and the imaginary part of the magnetic permeability of the ferrite material does not exceed 5 at 13.56MHz, and the real part of the magnetic permeability is greater than 235. In addition, due to the high cost of NiO, in the ferrite material of this embodiment, the NiO component is controlled below 9%, and can be as low as 7%. Compared with some existing ferrite materials, the NiO content is greatly reduced, thereby reducing the cost of the ferrite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present application, and are used together with the specification to explain the principles of the present application. In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor.

[0024] Figure 1 It is a schematic flow chart of a method for preparing a ferrite material provided in an embodiment of the present application;

[0025] Figure 2 is a cross-sectional view of the ferrite material of Example 1 of the present application;

[0026] Figure 3 This is a cross-sectional view of the ferrite material of Comparative Example 1.

[0027] The realization of the purpose, functional features and advantages of this application will be further described in conjunction with the embodiments and with reference to the accompanying drawings. The above-mentioned drawings have shown clear embodiments of this application, which will be described in more detail later. These drawings and textual descriptions are not intended to limit the scope of the concept of this application in any way, but to illustrate the concept of this application to those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION

[0028] As electronic products develop in the direction of being small, thin and light, the market has put forward higher requirements for magnetic sheets used for near-field communication antennas, requiring that the real part of the magnetic permeability of the magnetic sheet after fragmentation (including air gap) at a frequency of 13.56MHz should not be less than 180, and the imaginary part of the magnetic permeability should be less than 5. This requires that the real part of the magnetic permeability before the magnetic sheet is fragmented should be above 200, or even greater than 235, and the imaginary part of the magnetic permeability should be less than 5. The magnetic sheets made of existing ferrite materials either cannot meet the requirements in terms of real part of magnetic permeability, or the imaginary part of magnetic permeability exceeds 5, resulting in excessive loss. Based on this, the present application provides a ferrite material, a preparation method, a near-field communication antenna and a communication device.

[0029] The ferrite material provided in the embodiment of the present application includes a main component and an additive. The main component includes, by weight percentage, 60-70% Fe2O3, 15-22% ZnO, 7-10% CuO, and 7-9% NiO; based on the weight of the main component as 1, the additive includes: 0.6-1.0% Co2O3, and 0.2-0.4% LiF. For example, based on 100 parts by weight of the main component, the ferrite material may include the following components: 63 parts Fe2O3, 20 parts ZnO, 9 parts CuO, 8 parts NiO, 0.8 parts Co2O3, and 0.3 parts LiF.

[0030] The ferrite material of this embodiment is NiCuZn series. In order to meet the performance requirements of the NFC antenna, the content of each component has strict requirements. The influence of the content of each component on the performance is roughly as follows:

[0031] As for Fe2O3, Fe2O3 is a ferromagnetic material that helps to improve the magnetic moment of the material. If the content of Fe2O3 is less than 60wt%, the real part of the magnetic permeability of the obtained ferrite material at 13.56MHz cannot reach 235. If the content of Fe2O3 is higher than 70wt%, although the real part of the magnetic permeability of the ferrite material can meet the requirements (i.e., above 235), the imaginary part of the magnetic permeability is much greater than 5, which cannot meet the low loss requirements of the NFC antenna.

[0032] For ZnO, if the ZnO content is lower than 15wt%, the real part of the permeability of the ferrite material at 13.56MHz cannot reach 235. If the ZnO content is higher than 22wt%, although the real part of the permeability of the ferrite material meets the requirement, the imaginary part of the permeability is much larger than 5, which cannot meet the low loss requirement of the NFC antenna.

[0033] For CuO, if the CuO content is lower than 7wt%, the sintering activity of the ferrite material will be poor, resulting in low density after sintering, making it difficult to make the real part of the magnetic permeability of the ferrite material reach above 235 at 13.56MHz. If the CuO content is higher than 10wt%, the sintering activity of the ferrite material is too high, resulting in excessive growth of the material grains, which deteriorates the magnetic properties of the ferrite material and causes the imaginary part of the magnetic permeability to be much greater than 5, which cannot meet the low loss requirements.

[0034] For Co2O3, if the content of Co2O3 is lower than 0.6wt%, the imaginary part of the magnetic permeability of the ferrite material is much larger than 5, which cannot meet the low loss requirement of NFC. If the content of Co2O3 is higher than 1wt%, the real part of the magnetic permeability of the ferrite material at 13.56MHz is difficult to reach above 235.

[0035] As for LiF, LiF contains Li+ with a large ion radius and a small charge number, which is easy to occupy the B ion position of the spinel structure during the pre-sintering or sintering process of the ferrite material, forming more oxygen vacancy defects in the crystal structure, thereby easily reducing the pre-sintering temperature of the ferrite powder and playing a role in refining the grains, thereby improving the sintering activity of the ferrite material. If the content of LiF is less than 0.1wt%, it is difficult to play a role in refining the ferrite grains during the sintering process, thereby making it difficult to improve the sintering activity of the material. If the content of LiF is higher than 0.5wt%, the magnetic permeability of the ferrite material will be reduced.

[0036] It should be noted that when the ferrite material is sintered, if the grain growth of the ferrite material is not perfect, the real part of the magnetic permeability of the ferrite material is low; if the grains grow excessively, the magnetic properties of the ferrite material deteriorate, resulting in an imaginary part of the magnetic permeability greater than 5, which cannot meet the low loss requirements. The components of the ferrite material of this embodiment have strict ratio requirements, and the additives can improve the microstructure of the ferrite material during sintering (such as grain size, uniformity, density, etc.). Among them, Co2O3 has the effect of improving the high-frequency performance of the material, and cooperates with LiF to improve the green density of the ferrite material and achieve a semi-fused state of the grains, ultimately making the imaginary part of the magnetic permeability of the NiCuZn ferrite material of this embodiment not exceed 5 at 13.56MHz, and the real part of the magnetic permeability basically reaches a larger value, which can meet the requirement of being greater than 235.

[0037] In addition, due to the high cost of NiO, in the ferrite material of this embodiment, the NiO component is controlled below 9%, and according to research and test verification, the lowest can be 7%. Compared with some existing ferrite materials, the NiO content is greatly reduced, thereby reducing the cost of the ferrite material.

[0038] The present application also provides a method for preparing a ferrite material. Figure 1 , Figure 1 : is a schematic flow chart of a method for preparing a ferrite material provided in an embodiment of the present application, the method comprising:

[0039] S101. Ball-milling the main component and the additive to obtain a slurry, wherein the main component includes, by weight percentage, 60-70% Fe2O3, 15-22% ZnO, 7-10% CuO, and 7-9% NiO; based on the weight of the main component being 1, the additive includes, 0.6-1.0% Co2O3, and 0.2-0.4% LiF.

[0040] For example, the main component and the additive are first prepared according to the above components, and then the main component and the additive are mixed and ball-milled. As some examples, deionized water can be used as the solvent for ball milling, and the grinding body can be a zirconia ball with a diameter of 3 to 5 mm.

[0041] In one embodiment, the weight ratio of the total weight of the main component and the additive to the weight of the grinding body and water is 1:1:1. The rotation speed and milling time of the ball mill can be set according to the final powder particle size requirements. After the ball milling is completed, a slurry is obtained.

[0042] S102, sieving and pre-calcining the slurry to obtain a precursor powder.

[0043] For example, the obtained slurry can be dried first, for example, the slurry can be baked in an oven at 150° C. for 48 hours, and then sieved, for example, a 40-mesh sieve can be used to sieve, to obtain a uniform and fine primary powder, and then the primary powder is pre-calcined in an air atmosphere to obtain a precursor powder.

[0044] In one embodiment, the process conditions of pre-firing may be: pre-firing temperature is 785-815° C., and holding time is 100-150 min. The sintering activity of the precursor powder may be increased by pre-firing.

[0045] S103, pressing the precursor powder into a shape, and performing final sintering to obtain the ferrite material.

[0046] After the precursor powder is obtained, the precursor powder can be pressed into a shape. For example, compression molding can be used. As an example, the precursor powder can be placed in a mold of a preset shape, and then pressed at a temperature of 0.9 to 1.1 t / cm 2 The preset shape can be regarded as the shape of the precursor powder after being pressed and formed (for example, the obtained magnetic sheet).

[0047] The formed ferrite material is then subjected to final firing to obtain a finished product made of the ferrite material, such as a magnetic sheet. In one embodiment, the process conditions for final firing may be: a final firing temperature of 945 to 965° C. and a holding time of 100 to 150 minutes. For example, the formed ferrite material may be placed in a box-type sintering furnace at 950° C. and sintered for 2 hours.

[0048] The NiCuZn ferrite material prepared in this embodiment has an imaginary part of magnetic permeability less than 5 at 13.56 MHz, and a real part of magnetic permeability greater than 235. In addition, due to the low NiO content, the cost can be reduced at the same time.

[0049] The present application also provides a near field communication antenna, comprising a magnetic sheet, wherein the magnetic sheet comprises the ferrite material described in the above embodiments, or is prepared by the preparation method described in the above embodiments.

[0050] The embodiments of the present application also provide a communication device, which includes the near field communication antenna described in the above embodiments, so the communication device can also produce the beneficial effects of the near field communication antenna in each embodiment. As some examples, the communication device can be a mobile device such as a mobile phone, a smart watch / bracelet, a tablet computer, or a fixed device such as a router or a communication base station.

[0051] The present application is further described below with reference to specific embodiments.

[0052] Example 1

[0053] (1) Slurry preparation

[0054] The following raw materials were prepared in parts by weight: 63 parts of Fe2O3, 20 parts of ZnO, 9 parts of CuO, 8 parts of NiO, 0.8 parts of Co2O3 and 0.3 parts of LiF, and then ball-milled and mixed in a ratio of raw materials: grinding body: water = 1:1:1 to obtain a slurry.

[0055] (2) Preparation of precursor powder

[0056] The slurry was baked in an oven at 150°C for 48 hours, then sieved with a 40-mesh sieve, and finally the sieved powder was pre-sintered in an air atmosphere at a sintering temperature of 800°C and a sintering time of 120 minutes.

[0057] (3) Preparation of ferrite materials

[0058] The precursor powder is loaded into the mold and then 2 The ferrite material is formed by pressing under pressure and finally sintering at 955°C in an air atmosphere for 120 minutes and cooling in the furnace.

[0059] Example 2

[0060] (1) Slurry preparation

[0061] The following raw materials were prepared according to weight: 60 parts of Fe2O3, 22 parts of ZnO, 10 parts of CuO, 8 parts of NiO, 0.8 parts of Co2O3 and 0.3 parts of LiF, and then ball-milled and mixed according to the ratio of raw materials: grinding body: water = 1:1:1 to obtain a slurry.

[0062] (2) Preparation of precursor powder

[0063] The slurry was baked in an oven at 150°C for 48 hours, and then sieved with a 40-mesh sieve. Finally, the sieved powder was pre-calcined in an air atmosphere at a sintering temperature of 790°C and a sintering time of 140 minutes.

[0064] (3) Preparation of ferrite materials

[0065] The precursor powder is loaded into the mold and then 2 The ferrite material is formed by pressing under pressure and finally sintered in an air atmosphere at 960°C for 110 minutes. After cooling in the furnace, the ferrite material is prepared.

[0066] Example 3

[0067] (1) Slurry preparation

[0068] The following raw materials were prepared according to weight: 70 parts of Fe2O3, 15 parts of ZnO, 8 parts of CuO, 7 parts of NiO, 0.8 parts of Co2O3 and 0.3 parts of LiF, and then ball-milled and mixed according to the ratio of raw materials: grinding body: water = 1:1:1 to obtain a slurry.

[0069] (2) Preparation of precursor powder

[0070] The slurry was baked in an oven at 150°C for 48 hours, and then sieved with a 40-mesh sieve. Finally, the sieved powder was pre-sintered in an air atmosphere at a sintering temperature of 810°C and a sintering time of 110 minutes.

[0071] (3) Preparation of ferrite materials

[0072] The precursor powder is loaded into the mold and then 2 The ferrite material is formed by pressing under pressure and finally sintering in an air atmosphere at 950°C for 140 minutes and cooling in the furnace.

[0073] Example 4

[0074] (1) Slurry preparation

[0075] The following raw materials were prepared according to weight: 65 parts of Fe2O3, 18 parts of ZnO, 9 parts of CuO, 8 parts of NiO, 0.8 parts of Co2O3 and 0.3 parts of LiF, and then ball-milled and mixed according to the ratio of raw materials: grinding body: water = 1:1:1 to obtain a slurry.

[0076] (2) Preparation of precursor powder

[0077] The slurry was baked in an oven at 150°C for 48 hours, and then sieved with a 40-mesh sieve. Finally, the sieved powder was pre-sintered in an air atmosphere at a sintering temperature of 805°C and a sintering time of 120 minutes.

[0078] (3) Preparation of ferrite materials

[0079] The precursor powder is loaded into the mold and then 2 The ferrite material is formed by pressing under a pressure of 200°C and finally sintered in an air atmosphere at 952°C for 135 minutes. After cooling in the furnace, the ferrite material is prepared.

[0080] Example 5

[0081] (1) Slurry preparation

[0082] The following raw materials were prepared in parts by weight: 63 parts of Fe2O3, 20 parts of ZnO, 9 parts of CuO, 8 parts of NiO, 0.6 parts of Co2O3 and 0.4 parts of LiF, and then ball-milled and mixed in a ratio of raw materials: grinding body: water = 1:1:1 to obtain a slurry.

[0083] (2) Preparation of precursor powder

[0084] The slurry was baked in an oven at 150°C for 48 hours, then sieved with a 40-mesh sieve, and finally the sieved powder was pre-sintered in an air atmosphere at a sintering temperature of 800°C and a sintering time of 120 minutes.

[0085] (3) Preparation of ferrite materials

[0086] The precursor powder is loaded into the mold and then 2 The ferrite material is formed by pressing under pressure and finally sintering at 955°C in an air atmosphere for 120 minutes and cooling in the furnace.

[0087] Example 6

[0088] (1) Slurry preparation

[0089] The following raw materials were prepared according to weight: 63 parts of Fe2O3, 20 parts of ZnO, 9 parts of CuO, 8 parts of NiO, 1.0 parts of Co2O3 and 0.2 parts of LiF, and then ball-milled and mixed in a ratio of raw materials: grinding body: water = 1:1:1 to obtain a slurry.

[0090] (2) Preparation of precursor powder

[0091] The slurry was baked in an oven at 150°C for 48 hours, then sieved with a 40-mesh sieve, and finally the sieved powder was pre-sintered in an air atmosphere at a sintering temperature of 800°C and a sintering time of 120 minutes.

[0092] (3) Preparation of ferrite materials

[0093] The precursor powder is loaded into the mold and then 2 The ferrite material is formed by pressing under pressure and finally sintering at 955°C in an air atmosphere for 120 minutes and cooling in the furnace.

[0094] Comparative Example 1

[0095] Compared with Example 2, the only difference is that the raw material formula is: 55 parts of Fe2O3, 28 parts of ZnO, 10 parts of CuO, 7 parts of NiO, 0.8 parts of Co2O3 and 0.3 parts of LiF.

[0096] Comparative Example 2

[0097] Compared with Example 1, the only difference is that the raw material formula is: 74 parts of Fe2O3, 7 parts of ZnO, 6 parts of CuO, 13 parts of NiO, 0.8 parts of Co2O3 and 0.3 parts of LiF.

[0098] The raw material components of the above embodiments and comparative examples are specifically shown in Table 1 below.

[0099] Table 1 Raw material components and performance test data of each embodiment and comparative example

[0100]

[0101] Performance testing and morphology characterization

[0102] The samples of Example 1 and Comparative Example 1 were subjected to SEM test, wherein: Figure 2 is a cross-sectional view of the ferrite material of Example 1 of the present application, wherein the grain size of the ferrite material is uniform and dense; Figure 3 It is a cross-sectional view of the ferrite material of comparative example 1. The ferrite material has coarse grains and many voids.

[0103] The real part (u') and imaginary part (u") of the magnetic permeability of the magnetic sheet samples made in each embodiment and comparative example were tested using Keysight 4990 radio frequency impedance analyzer. The test results are shown in Table 1.

[0104] It can be seen from the data in Table 1 that the magnetic properties of the ferrite materials prepared in Examples 1 to 6 of the present application all meet the following requirements: the real part of the magnetic permeability is greater than 235, and the imaginary part of the magnetic permeability is less than 5. In addition, the comprehensive performance of the ferrite material in Example 1 is the best.

[0105] Compared with Example 1, the components of Control Example 1 and Control Example 2 exceed the range specified in this application. The real part of the magnetic permeability of the ferrite material of Control Example 1 is lower than 235, and the imaginary part of the magnetic permeability of the ferrite material of Control Example 2 is greater than 5.

[0106] The above is a detailed introduction to a ferrite material, a preparation method, a near-field communication antenna and a communication device provided by the present application. This article uses specific examples to illustrate the principles and implementation methods of the present application. It should be noted that in the present application, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, please refer to the relevant description of other embodiments.

[0107] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a ferrite material, characterized in that: include: The main component and the additive are ball-milled to obtain a slurry, wherein the main component comprises, by weight percentage, 63% of Fe2O3, 20% of ZnO, 9% of CuO, and 8% of NiO; based on the weight of the main component being 1, the additive comprises, 0.8% of Co2O3, and 0.3% of LiF; The slurry is dried, then sieved through 40 meshes, and pre-calcined to obtain a precursor powder; The precursor powder is placed in a mold, and then pressed into shape at a pressure of 1.0, and finally fired to obtain the ferrite material, the final firing temperature is 955° C., and the holding time is 120 min; In the pre-firing step, the pre-firing temperature is 800°C and the holding time is 120 minutes; In the ball milling step, the weight ratio of the total weight of the main component and the additive to the grinding body and water is 1:1:

1.

2. A ferrite material, characterized in that: The preparation method according to claim 1 is used for preparation.

3. A near field communication antenna, comprising a magnetic sheet, characterized in that: The magnetic sheet comprises the ferrite material according to claim 2.

4. A communication device, characterized in that: Includes the near field communication antenna as claimed in claim 3.