A composite antioxidant for extending the induction period of lubricating oil and a preparation method thereof
Patent Information
- Application Number
- CN202310282441.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-22
AI Technical Summary
In areas with large temperature differences between day and night, the solubility and dispersion of antioxidants in lubricating oil are easily imbalanced, making it difficult to exert stable antioxidant properties during application and affecting the service life of the lubricating oil.
A composite antioxidant is used, including organophosphorus compounds, tert-butyl-p-diphenol, amine antioxidants, zinc dialkyl dithiophosphates and benzodiazole, and the antioxidant modification auxiliary is prepared. It forms a stable antioxidant matrix and maintains the balance of solubility and dispersion by adjusting the bridge function in high and low temperature environments, extending the induction period of lubricating oil.
It effectively extends the service life of lubricating oil, improves the anti-oxidation performance, can slow down thermal degradation in high-temperature environments, and maintains good dispersion and molecular mobility in low-temperature environments, significantly improving the application stability of lubricating oils.
Smart Images

Figure BDA0004138493650000051 
Figure BDA0004138493650000061 
Figure BDA0004138493650000091
Abstract
Description
Technical Field
[0001] The present application relates to the field of antioxidants, and more specifically, to a composite antioxidant for extending the induction period of lubricating oil and a preparation method thereof. Background Art
[0002] Antioxidants in lubricating oil can be divided into three types according to their mechanism of action: free radical terminators, peroxide decomposers and metal deactivators. These types of antioxidants play a positive role in improving the quality of lubricating oil, enhancing the antioxidant properties of oil products and extending the service life of oil products. With the development of lubricating oil and additive technology, more and more environmentally friendly, complex, efficient and multifunctional antioxidants have been gradually developed to adapt to the progress of the times and environmental protection requirements.
[0003] The Chinese invention patent application document with publication number CN104059715A discloses an antioxidant composition, a lubricating oil composition and a method for improving the antioxidant performance of a lubricating oil. The antioxidant composition comprises alkylphenylnaphthylamine, phenothiazine and sulfurized hindered phenol, and the lubricating oil composition obtained by using the antioxidant composition has the advantages of low sulfur, low ash, phosphorus-free and good thermal stability, can significantly improve the oxidation stability of the lubricating oil under high temperature conditions and metal ion catalysis conditions, effectively extend the service life of the lubricating oil, and can effectively control the generation trend of deposits under high temperature conditions, meeting the requirements for the preparation of high-grade lubricating oils.
[0004] With respect to the above-mentioned related technologies, the inventors believe that antioxidants extend the service life of lubricants by extending the induction period of lubricants. However, in areas with large temperature differences between day and night, due to the frequent alternation of hot and cold, the solubility and dispersibility of antioxidants in lubricants are prone to imbalance, resulting in difficulty in exerting stable antioxidant properties during the application process. Therefore, it is urgently necessary to propose a solution to solve the above-mentioned technical problems. Summary of the invention
[0005] In order to enable the antioxidant to play a stable role in lubricating oil in areas with large temperature differences between day and night, the present application provides a composite antioxidant for extending the induction period of lubricating oil and a preparation method thereof.
[0006] In a first aspect, the present application provides a composite antioxidant for extending the induction period of lubricating oil, using the following technical solution:
[0007] A composite antioxidant for extending the induction period of lubricating oil, comprising the following components in parts by weight:
[0008] 10-40 parts of an organophosphorus compound;
[0009] 5-10 parts of tert-butyl p-diphenol;
[0010] 5-10 parts of amine antioxidant;
[0011] 5-10 parts of zinc dialkyl dithiophosphate;
[0012] 1-10 parts of benzodiazepine;
[0013] Dispersant 5-12 parts;
[0014] 0.5-2.5 parts of antioxidant modification additive;
[0015] The antioxidant modification aid is prepared by the following steps:
[0016] S1. Mix 2,6-di-tert-butyl-p-nitrophenol and anhydrous ethanol in a weight ratio of 1:(15-25) to obtain a mixed solution;
[0017] S2, adding 1.2-1.5 times the amount of the mixed solution of the modifying agent, the modifying agent is composed of calcium chloride solution and zinc powder in a weight ratio of (10-15): 1, then heating to 60-80 ° C, reflux for 6-8h, to obtain a reaction mixture;
[0018] S3. After cooling the reaction mixture, filter it under negative pressure to obtain a solid product, wash it with deionized water, and dry it in vacuum to obtain an antioxidant modified auxiliary agent.
[0019] By adopting the above technical scheme, due to the use of organic phosphorus compounds, tert-butyl para-diphenol, amine antioxidants, zinc dialkyl dithiophosphates and benzodiazepines, they cooperate with each other to form an excellent and stable antioxidant substance, and can exert an excellent antioxidant effect when applied to lubricating oil. The antioxidant modified auxiliary agent prepared by this application can, on the one hand, exert an excellent compound synergistic effect with the antioxidant substance formed by other antioxidant components, so that the composite antioxidant can exert a significant and outstanding antioxidant effect when applied to lubricating oil; on the other hand, when the composite antioxidant is in an area with a large temperature difference between day and night and is affected by frequent alternation of hot and cold, the antioxidant modified auxiliary agent can act as a regulating bridge between the molecules of other antioxidant components. When the composite antioxidant is applied to lubricating oil, it can greatly slow down the thermal degradation of its own antioxidant components in a high temperature environment, and can maintain good dispersibility and molecular mobility in a low temperature environment. It can also be adaptively adjusted as the lubricating oil's own characteristics change during heating and cooling, and the solubility and dispersibility remain relatively balanced, thereby playing an excellent and stable role in extending the induction period of the lubricating oil, effectively extending the service life of the lubricating oil, and the overall application effect is outstanding and significant.
[0020] Preferably, the components of the composite antioxidant for extending the induction period of lubricating oil also include 5-8 parts by weight of a regulating aid, the regulating aid is composed of poly-p-methoxyphenol and styrene-fumarate copolymer, and the weight ratio of poly-p-methoxyphenol to styrene-fumarate copolymer is 1:(2.1-3.5).
[0021] By adopting the above technical scheme, the thermal stability of poly-p-methoxyphenol can exert excellent antioxidant performance in a high temperature environment; styrene-fumarate copolymer enables the composite antioxidant to maintain good dispersion stability in a low temperature environment; and the adjustment auxiliary agent composed of poly-p-methoxyphenol and styrene-fumarate copolymer in a specific proportion can further improve the application stability of the composite antioxidant in high and low temperature environments. At the same time, the combination of poly-p-methoxyphenol and styrene-fumarate copolymer can enhance the role of antioxidant modification auxiliary agents, and they can be compounded and enhanced with each other, greatly improving the antioxidant effect of the composite oxidant in the application of lubricating oil, and in view of the frequent alternation of cold and hot caused by the large temperature difference between day and night, the composite oxidant can also play a better role and maintain a relatively excellent and stable application effect.
[0022] Preferably, the weight ratio of the poly-p-methoxyphenol to the styrene-fumarate copolymer is 1:3.
[0023] By adopting the above technical scheme, the combined dispersion state formed by the poly(p-methoxyphenol) and styrene-fumarate copolymer in the above weight ratio and the other component raw materials is relatively uniform and stable, and can thus exert a relatively excellent coordination effect, so that the composite oxidant used in lubricating oil can better cope with the adverse effects of frequent alternation of hot and cold, and show excellent and stable antioxidant properties.
[0024] Preferably, the average molecular weight of the poly(p-methoxyphenol) is 800-1100, and the average molecular weight of the styrene-fumarate copolymer is 5000-10000.
[0025] By adopting the above technical scheme, the poly-p-methoxyphenol and styrene-fumarate copolymer with the above molecular weight has excellent dispersibility stability in the composite oxidant, and can thus exert a relatively excellent coordination effect, and can form a uniform and stable combination with the antioxidant modification auxiliary agent, and play a relatively outstanding and excellent composite synergistic effect with each other.
[0026] Preferably, the organophosphorus compound is one or a combination of phosphite, triphenyl phosphite, alkyl phosphite and alkyl phosphite.
[0027] By adopting the above technical scheme, the above-mentioned types of organic phosphorus compounds have excellent anti-wear effects when in contact with relatively rough friction surfaces and slowly sliding metal surfaces, can eliminate peroxyl radicals and alkoxyl radicals, and can inhibit photodegradation, thereby effectively delaying the oxidation rate of the lubricating oil, increasing the service life of the lubricating oil, and being beneficial to energy saving and consumption reduction.
[0028] Preferably, the amine antioxidant is one or a combination of dialkyldiphenylamine, dialkylphenyldiphenylamine and dialkylbenzyldiphenylamine.
[0029] By adopting the above technical scheme, the above-mentioned type of amine antioxidant has excellent antioxidant and anti-corrosion capabilities and good anti-coking effect. When used in lubricating oil, it can effectively prevent the formation of sludge, thereby ensuring that the lubricating oil has a longer service life.
[0030] Preferably, the dispersant is one or a combination of succinimide, polyisobutylene succinimide and isobutylene succinate.
[0031] By adopting the above technical scheme, the above type of dispersant can not only make the various component raw materials fully mixed to obtain a composite antioxidant of excellent quality, but also can disperse the dirt in the oil during the application of the antioxidant to prevent the dirt from forming precipitation, thereby ensuring that its own antioxidant effect can be stably and excellently exerted.
[0032] In a second aspect, the present application provides a method for preparing a composite antioxidant for prolonging the induction period of lubricating oil, using the following technical solution:
[0033] A method for preparing a composite antioxidant for extending the induction period of lubricating oil comprises the following steps:
[0034] (1) Prepare raw materials including an organic phosphorus compound, tert-butyl para-diphenol, an amine antioxidant, zinc dialkyl dithiophosphate, benzodiazepine, a dispersant and an antioxidant modification aid according to a ratio.
[0035] (2) The organic phosphorus compound, tert-butyl para-diphenol, amine antioxidant, zinc dialkyl dithiophosphate and benzodiazepine in step (1) are mixed, heated to 40-60° C. under normal pressure, stirred evenly while keeping warm, and then a dispersant and an antioxidant modification aid are added, and the stirring is continued while keeping warm and evenly, thereby obtaining a composite antioxidant for extending the induction period of lubricating oil.
[0036] By adopting the above technical solution, the preparation steps of the composite antioxidant of the present application are relatively few, the process is simple, and it is convenient for large-scale production. At the same time, during the preparation process, the material is added and stirred twice, which is conducive to quality control during the process, and the dispersant and the antioxidant modification auxiliary agent are added last, which is conducive to fully combining the antioxidant modification auxiliary agent with other raw materials, thereby being able to obtain a composite antioxidant with stable and excellent quality that prolongs the induction period of lubricating oil.
[0037] In summary, this application has the following beneficial effects:
[0038] 1. Since the antioxidant modified additive prepared in the present application is not only fully compounded with the antioxidant substances formed by other antioxidant components to enhance the synergy, but also can act as a regulating bridge between the molecules of other antioxidant components, so that when the obtained composite antioxidant is applied to lubricating oil, it can well cope with the high and low temperature changes caused by environmental influences, and its solubility and dispersibility are relatively balanced during the process, which can effectively extend the service life of the lubricating oil and is conducive to energy saving and consumption reduction;
[0039] 2. The present application adopts the use of poly-p-methoxyphenol and styrene-fumarate copolymer in a specific proportion to form an adjusting auxiliary agent, which can enhance and promote the effect of the antioxidant modification auxiliary agent, and can be compounded with each other to enhance the synergy, thereby further improving the application stability of the composite antioxidant in high and low temperature environments, which is beneficial to greatly extend the induction period of the lubricant, delay the oxidation rate of the lubricant, and effectively extend the service life of the lubricant. DETAILED DESCRIPTION
[0040] The present application is further described in detail below with reference to the embodiments.
[0041] Unless otherwise specified, the raw materials used in the embodiments of the present application are commercially available.
[0042] Preparation examples of raw materials and / or intermediates
[0043] Preparation Example 1
[0044] An antioxidant modification auxiliary agent is prepared by the following steps:
[0045] S1. Mix 2,6-di-tert-butyl-p-nitrophenol and anhydrous ethanol in a weight ratio of 1:20 to obtain a mixed solution;
[0046] S2, adding a modifying agent 1.35 times the amount of the mixed solution, the modifying agent consisting of a calcium chloride solution and zinc powder in a weight ratio of 12.5:1, then heating to 70° C., reflux for 7 hours, to obtain a reaction mixture;
[0047] S3. After cooling the reaction mixture, filter it under negative pressure to obtain a solid product, wash it with deionized water, and vacuum dry it at 40° C. for 24 hours to obtain an antioxidant modification auxiliary agent.
[0048] Note: The mass fraction of calcium chloride solution in the above steps is 20%.
[0049] Preparation Example 2
[0050] An antioxidant modification auxiliary agent is prepared by the following steps:
[0051] S1. Mix 2,6-di-tert-butyl-p-nitrophenol and anhydrous ethanol in a weight ratio of 1:15 to obtain a mixed solution;
[0052] S2, adding a modifying agent of 1.2 times the amount of the mixed solution, wherein the modifying agent is composed of a calcium chloride solution and zinc powder in a weight ratio of 10:1, and then heating to 60° C. and reflux for 8 hours to obtain a reaction mixture;
[0053] S3. After cooling the reaction mixture, filter it under negative pressure to obtain a solid product, wash it with deionized water, and vacuum dry it at 40° C. for 24 hours to obtain an antioxidant modification auxiliary agent.
[0054] Preparation Example 3
[0055] An antioxidant modification auxiliary agent is prepared by the following steps:
[0056] S1. Mix 2,6-di-tert-butyl-p-nitrophenol and anhydrous ethanol in a weight ratio of 1:25 to obtain a mixed solution;
[0057] S2, adding a modifying agent 1.5 times the amount of the mixed solution, the modifying agent consisting of a calcium chloride solution and zinc powder in a weight ratio of 15:1, then heating to 80° C., reflux for 6 hours, to obtain a reaction mixture;
[0058] S3. After cooling the reaction mixture, filter it under negative pressure to obtain a solid product, wash it with deionized water, and vacuum dry it at 40° C. for 24 hours to obtain an antioxidant modification auxiliary agent.
[0059] Example
[0060] Example 1
[0061] A composite antioxidant for extending the induction period of lubricating oil, the raw materials of each component and their corresponding weights are shown in Table 1, and is prepared by the following steps:
[0062] (1) Prepare raw materials including an organic phosphorus compound, tert-butyl para-diphenol, an amine antioxidant, zinc dialkyl dithiophosphate, benzodiazepine, a dispersant and an antioxidant modification aid according to a ratio.
[0063] (2) The organic phosphorus compound, tert-butyl para-diphenol, amine antioxidant, zinc dialkyl dithiophosphate and benzodiazepine in step (1) are mixed, heated to 40-60° C. (preferably 50° C. in this embodiment) under normal pressure, stirred evenly while keeping warm, stirred at 300 r / min for 30 min, and then a dispersant and an antioxidant modification aid are added, and the mixture is stirred evenly while keeping warm, and stirred at 300 r / min for 10 min to obtain a composite antioxidant for extending the induction period of lubricating oil.
[0064] Note: In the above steps, the organic phosphorus compound is phosphite. The amine antioxidant is dialkyl diphenylamine. The dispersant is succinimide. The antioxidant modification aid is obtained in Preparation Example 1.
[0065] Example 2-3
[0066] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the raw materials of its components and their corresponding weights are shown in Table 1.
[0067] Table 1 Raw materials of each component in Examples 1-3 and their weight parts (kg / part)
[0068]
[0069]
[0070] Example 4
[0071] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the organic phosphorus compound is a composition of triphenyl phosphite and alkyl phosphite in a weight ratio of 1:1.
[0072] Example 5
[0073] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the amine antioxidant is a composition of dialkylphenyl diphenylamine and dialkylbenzyl diphenylamine in a weight ratio of 1:1.
[0074] Example 6
[0075] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the dispersant is a composition of polyisobutylene succinimide and isobutylene succinate in a weight ratio of 1:1.
[0076] Example 7
[0077] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that when the antioxidant modification aid is added for use, 6.5 parts of a regulating aid are added simultaneously, and the regulating aid is composed of poly-p-methoxyphenol and styrene-fumarate copolymer in a weight ratio of 1:3; wherein the average molecular weight of the poly-p-methoxyphenol is 950, and the average molecular weight of the styrene-fumarate copolymer is 7500.
[0078] Example 8
[0079] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the weight portion of the regulating auxiliary agent added is 5 parts.
[0080] Example 9
[0081] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the weight portion of the regulating auxiliary agent added is 8 parts.
[0082] Example 10
[0083] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the regulating auxiliary agent is composed of poly-p-methoxyphenol and styrene-fumarate copolymer in a weight ratio of 1:2.1.
[0084] Embodiment 11
[0085] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the regulating auxiliary agent is composed of poly-p-methoxyphenol and styrene-fumarate copolymer in a weight ratio of 1:3.5.
[0086] Example 12
[0087] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the regulating auxiliary agent is composed of poly-p-methoxyphenol and styrene-fumarate copolymer in a weight ratio of 1:2.8.
[0088] Embodiment 13
[0089] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the average molecular weight of poly-p-methoxyphenol is 800, and the average molecular weight of styrene-fumarate copolymer is 5000.
[0090] Embodiment 14
[0091] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the average molecular weight of poly-p-methoxyphenol is 1100, and the average molecular weight of styrene-fumarate copolymer is 10000.
[0092] Embodiment 15
[0093] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the mass of poly-p-methoxyphenol is replaced by styrene-fumarate copolymer.
[0094] Example 16
[0095] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the styrene-fumarate copolymer is replaced by poly-p-methoxyphenol in equal mass.
[0096] Embodiment 17
[0097] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the regulating auxiliary agent is composed of poly-p-methoxyphenol and styrene-fumarate copolymer in a weight ratio of 1:2.
[0098] Embodiment 18
[0099] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the regulating auxiliary agent is composed of poly-p-methoxyphenol and styrene-fumarate copolymer in a weight ratio of 1:3.6.
[0100] Embodiment 19
[0101] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the average molecular weight of poly-p-methoxyphenol is 700, and the average molecular weight of styrene-fumarate copolymer is 4500.
[0102] Embodiment 20
[0103] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the average molecular weight of poly-p-methoxyphenol is 1200, and the average molecular weight of styrene-fumarate copolymer is 10500.
[0104] Embodiment 21
[0105] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the antioxidant modification auxiliary agent is obtained in Preparation Example 2.
[0106] Embodiment 22
[0107] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the antioxidant modification auxiliary agent is obtained in Preparation Example 3.
[0108] Comparative Example
[0109] Comparative Example 1
[0110] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the raw material does not contain an antioxidant modification aid.
[0111] Comparative Example 2
[0112] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 1 in that the antioxidant modification auxiliary agent is replaced by 2,6-di-tert-butyl-p-nitrophenol.
[0113] Comparative Example 3
[0114] A composite antioxidant for extending the induction period of lubricating oil, which is different from Example 7 in that the raw material does not contain an antioxidant modification aid.
[0115] Performance test samples: The composite antioxidant for extending the induction period of lubricating oil obtained in Examples 1-22 was used as test sample 1-22, and the composite antioxidant for extending the induction period of lubricating oil obtained in Comparative Examples 1-3 was used as control sample 1-3.
[0116] Test method: Take three commercially available lubricants, namely Qiongtian Zhuoli L-AN46 mechanical lubricant, Apex APEX FM S320 food grade fully synthetic lubricant, and Zhuobao L-CKC150 industrial gear oil;
[0117] Take 25 portions of each lubricating oil, each portion of lubricating oil is 500 ml, and take 1 portion of each of the three lubricating oils as a group, and divide into 25 groups in total; add test samples 1-22 and control samples 1-3 to the 25 groups of lubricating oils respectively, wherein 0.3% by weight of the composite antioxidant is added to each lubricating oil, and 25 groups of test oils can be obtained;
[0118] Take half of each of the 25 test oils, and measure the oxidation induction period of the three lubricating oils using the standard SH / T 0719-2002 "Determination of oxidation induction period of lubricating oil (pressure differential scanning calorimetry)", and take the average value, which is recorded as the initial average oxidation induction period;
[0119] Take the remaining half of the 25 groups of test oils, put them into a high and low temperature cycle test box, heat them to 40°C at 2°C / min, keep them warm for 10 hours, then cool them to -10°C at 1°C / min, keep them warm for 6 hours, then heat them to 25°C at 2°C / min, keep them warm for 2 hours, which is recorded as one cycle; after completing 7 cycles, take out the 25 groups of test oils, and measure the oxidation induction period of the three lubricating oils using the standard SH / T 0719-2002 "Determination of oxidation induction period of lubricating oil (pressure differential scanning calorimetry)", take the average value, and record it as the average oxidation induction period after the test;
[0120] The reduction rate of the oxidation induction period was calculated, where the reduction rate of the oxidation induction period = (initial average oxidation induction period - average oxidation induction period after the test) / initial average oxidation induction period. The lower the reduction rate of the oxidation induction period, the less affected it is by the external temperature change environment. The reduction rates of the oxidation induction period obtained for the 25 groups of test oils are recorded in Table 2 for the test samples 1-22 and the control samples 1-3.
[0121] Table 2 Test results of test samples 1-22 and control samples 1-3
[0122]
[0123]
[0124] Combining Examples 1-3, Examples 21-22 and Comparative Examples 1-2 and Table 2, it can be seen that the antioxidant modification additive prepared in the present application can greatly improve the high and low temperature resistance of the composite antioxidant in the lubricating oil, and the oxidation induction period reduction rate obtained in the test process is relatively low. Although the use of untreated 2,6-di-tert-butyl-p-nitrophenol can reduce the oxidation induction period reduction rate, the effect is far less than that of the prepared antioxidant modification additive.
[0125] It can be seen from Example 1 and Example 7-12 and Table 2 that the present application uses poly-p-methoxyphenol and styrene-fumarate copolymer as a regulating aid in a specific ratio, which can further improve the application stability of the composite antioxidant in a high and low temperature environment, greatly reduce the oxidation induction period reduction rate, and thus be more conducive to delaying the oxidation rate of the lubricating oil. Among them, when the weight ratio of poly-p-methoxyphenol and styrene-fumarate copolymer is 1:3, the improvement effect is the most excellent. It can be seen from Example 15-16 and Table 2 that poly-p-methoxyphenol and styrene-fumarate copolymer can play a composite synergistic effect. Using poly-p-methoxyphenol or styrene-fumarate copolymer as a regulating aid alone has limited effects, and is far less than the excellent effect of the composite of the two. Only when the two are composited, the measured oxidation induction period reduction rate is the lowest, indicating that it can play an excellent and stable effect in an environment with high and low temperature changes, and its application is outstanding.
[0126] Combined with Examples 17-18 and Table 2, it can be seen that when the weight ratio of poly-p-methoxyphenol and styrene-fumarate copolymer is lower than or higher than 1: (2.1-3.5), the lifting effect is limited and far from the compounding synergistic effect in Example 1. Combined with Examples 13-14, Examples 19-20 and Table 2, it can be seen that when the average molecular weight of poly-p-methoxyphenol is 800-1100 and the average molecular weight of styrene-fumarate copolymer is 5000-10000, it is more conducive to compounding the two and exerting excellent lifting effect, while when it is lower than or higher than the above molecular weight range, the lifting effect is limited and far less than Example 1, which may be caused by the low stability of the intermolecular binding, which is easily destroyed in the environment of high and low temperature changes, and the antioxidant effect is limited.
[0127] It can be seen from Example 1, Example 7, Comparative Example 1 and Comparative Example 3 and Table 2 that the regulating auxiliary agent and the antioxidant modifying auxiliary agent, when mixed and used, have a compounding and synergistic effect with each other, and can achieve the technical effect of 1+1>2, so that when the composite oxidant is used in the lubricating oil, it can well cope with the high and low temperature changes caused by environmental influences, and its own solubility and dispersibility remain relatively balanced during the process, which can effectively extend the service life of the lubricating oil.
[0128] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A composite antioxidant for extending the induction period of lubricating oil, Features: Contains the following components in parts by weight: 10-40 parts of an organophosphorus compound; 5-10 parts of tert-butyl p-diphenol; 5-10 parts of amine antioxidant; 5-10 parts of zinc dialkyl dithiophosphate; 1-10 parts of benzodiazepine; Dispersant 5-12 parts; 0.5-2.5 parts of antioxidant modification additive; The antioxidant modification aid is prepared by the following steps: S1. Mix 2,6-di-tert-butyl-p-nitrophenol and anhydrous ethanol in a weight ratio of 1:(15-25) to obtain a mixed solution; S2, adding a modifying agent of 1.2-1.5 times the amount of the mixed solution, wherein the modifying agent is composed of a calcium chloride solution and zinc powder in a weight ratio of (10-15):1, then heating to 60-80°C, reflux for 6-8h, and obtaining a reaction mixture; S3, after cooling the reaction mixture, filtering under negative pressure to obtain a solid product, washing with deionized water, and vacuum drying to obtain an antioxidant modification additive; The composite antioxidant for extending the induction period of lubricating oil further comprises 5-8 parts by weight of a regulating aid, the regulating aid being composed of poly-p-methoxyphenol and styrene-fumarate copolymer, and the weight ratio of poly-p-methoxyphenol to styrene-fumarate copolymer is 1:(2.1-3.5); The average molecular weight of the poly-p-methoxyphenol is 800-1100, and the average molecular weight of the styrene-fumarate copolymer is 5000-10000.
2. The composite antioxidant for extending the induction period of lubricating oil according to claim 1, Features: The weight ratio of the poly-p-methoxyphenol to the styrene-fumarate copolymer is 1:
3.
3. The composite antioxidant for extending the induction period of lubricating oil according to claim 1, Features: The organic phosphorus compound is one or a combination of phosphite, triphenyl phosphite and alkyl phosphite.
4. The composite antioxidant for extending the induction period of lubricating oil according to claim 1, Features: The amine antioxidant is one or a combination of dialkyl diphenylamine, dialkyl phenyl diphenylamine and dialkyl benzyl diphenylamine.
5. The composite antioxidant for extending the induction period of lubricating oil according to claim 1, Features: The dispersant is one or a combination of succinimide, polyisobutylene succinimide and isobutylene succinate.
6. The method for preparing the composite antioxidant for extending the induction period of lubricating oil according to claim 1, Features: The following steps are involved: (1) preparing raw materials including an organophosphorus compound, tertiary butyl paradiphenol, an amine antioxidant, zinc dialkyl dithiophosphate, benzodiazepine, a dispersant, an antioxidant modification aid and a regulating aid according to a proportion; (2) The organic phosphorus compound, tert-butyl-p-diphenol, amine antioxidant, zinc dialkyl dithiophosphate and benzodiazepine in step (1) are mixed, heated to 40-60° C. under normal pressure, stirred evenly while keeping warm, and then a dispersant, an antioxidant modification aid and a regulating aid are added, and the mixture is stirred evenly while keeping warm, thereby obtaining a composite antioxidant for extending the induction period of lubricating oil.