A low-chlorine high-aluminum correction material based on recycled aluminum secondary aluminum ash, production and use

By performing hydrolysis and washing in an integrated hydrolysis, washing and filtering tank, a low-chlorine and high-aluminum calibration material is generated, which solves the dual needs of low-chlorine and high-aluminum recycled aluminum secondary aluminum ash in Portland cement production and achieves resource efficiency. Utilize and environmentally friendly production processes.

CN116375367BActive Publication Date: 2024-10-29FUJIAN RONGCHANGDA ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310116672.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-15
Publication Date
2024-10-29
Estimated Expiration
2043-02-15

AI Technical Summary

Technical Problem

It is difficult to use recycled aluminum secondary aluminum ash to achieve the dual requirements of low chlorine and high aluminum in Portland cement production with existing technology, and existing treatment methods have problems such as high energy consumption and dust pollution.

Method used

A hydrolysis, washing and filtration integrated tank is used to hydrolyze aluminum nitride and wash and filter to remove chlorine salts to generate low-chlorine and high-aluminum calibration materials. Ammonium sulfate is recovered through an ammonia absorption step, and the salt-containing solution is further processed to improve resource utilization.

Benefits of technology

It achieves efficient utilization of aluminum correction raw materials in the production of Portland cement and clay sintered bricks, reduces chloride ion content and energy consumption, avoids dust pollution, and improves production efficiency and resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116375367B_ABST
    Figure CN116375367B_ABST
Patent Text Reader

Abstract

This invention relates to the field of comprehensive utilization technology of recycled aluminum secondary aluminum ash, and more specifically to a low-chlorine, high-alumina correcting material based on recycled aluminum secondary aluminum ash, its production, and applications. By employing an integrated hydrolysis-washing-filtration tank, and performing hydrolysis to remove aluminum nitride and washing to remove chloride salts within it, the recycled aluminum secondary aluminum ash raw material undergoes "fully enclosed," "one-stop" stirring, hydrolysis, washing, and filtration in the integrated hydrolysis-washing-filtration tank. This reduces the aluminum nitride content to below 1%, the chloride ion content to below 0.06%, and increases the aluminum oxide content to over 75%, with a moisture content below 10%. This meets the standards for aluminum correcting materials used in the production of silicate cement and clay sintered bricks, achieving the harmless treatment and resource utilization of secondary aluminum ash. The production method of this invention allows for the on-site deployment of relevant treatment equipment at the generation site of the secondary aluminum ash, enabling on-site harmless treatment of the ash without secondary pollution such as fugitive emissions of dust, ammonia, or other harmful gases, making it clean and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of comprehensive utilization of secondary aluminum ash of recycled aluminum, and more specifically relates to a low-chlorine and high-aluminum correction material based on secondary aluminum ash of recycled aluminum, and its production and use. Background Art

[0002] Recycled aluminum is the aluminum and aluminum alloy produced by smelting with scrap aluminum as the main raw material. In the smelting process, a flux composed of NaCl, KCl, etc. should be used to melt the scrap aluminum under the coverage of the flux layer to ensure that the recycled aluminum has a high recovery rate and quality. The secondary aluminum ash produced by the aluminum ash slag produced on the surface of the scrap aluminum and aluminum ingots during remelting, refining, alloying, and casting melts after the aluminum is recovered is listed as a hazardous waste in the "National List of Hazardous Wastes". The waste category is HW48 non-ferrous metal mining and smelting waste, the waste code is 321-026-48, and the hazardous characteristic is reactivity.

[0003] The aluminum nitride content in secondary aluminum ash is generally 10%-30%, and it is relatively active. It is easy to undergo hydrolysis reaction in water to generate ammonia, which is harmful to both people and the environment. However, since secondary aluminum ash still contains 2%-8% metallic aluminum, 45%-55% aluminum oxide, 15%-25% flux salts and other components, if it is not used reasonably, it will not only be a serious waste of the resources contained in the secondary aluminum ash, but also cause serious pollution to the environment. Therefore, eliminating the hazardous waste characteristics of secondary aluminum ash from recycled aluminum and removing aluminum nitride have become important issues for the harmless treatment of secondary aluminum ash from recycled aluminum and further its comprehensive resource utilization.

[0004] In the production of silicate cement, in order to improve the fluctuation of components from raw materials and fuels, it is often necessary to add high-grade aluminum correction raw materials and high-priced bauxite, which leads to high energy consumption and cost of cement clinker production industry, and faces the situation of being eliminated under the general environment of energy saving, consumption reduction and emission reduction. Therefore, an important direction of the comprehensive utilization of secondary aluminum ash resources is to use it as aluminum correction raw materials in the silicate cement production industry. For example, the patent document with patent number CN114524630B discloses "a method of using aluminum ash as fuel, correction material and combustion aid for dry cement production", and aluminum ash and catalytic combustion promoter are mixed in the conveying pipeline or in the burner, and sprayed into the decomposition furnace at the end of the kiln of the dry cement production line through the injection pipe or the burner. Under the catalytic activation of the catalytic combustion promoter, it is quickly burned out in a suspended state within 3 seconds to 8 seconds in a high temperature environment of 850℃ to 1200℃, and the activated alumina produced by the combustion is directly used as the aluminum correction raw material of the raw material. However, the aluminum ash in this method is primary aluminum ash or / and secondary aluminum ash treated with primary aluminum ash by a salt-free process, or secondary aluminum ash obtained by treating primary aluminum ash by a molten salt process. In this method, it is necessary to ensure that the aluminum ash is a high-grade aluminum correction raw material. For secondary aluminum ash raw materials with salt content still as high as 5%-25%, the addition ratio of secondary aluminum ash should be as low as possible to ensure that the chloride ion content in the cement clinker obtained by the final calcination does not exceed 0.06%. However, this method obviously cannot balance the dual requirements of aluminum correction raw materials for "high aluminum" and "low chlorine" content. Lou Meishan et al. also introduced the use of untreated industrial aluminum ash directly as an aluminum correction raw material for cement clinker production in "Application of Industrial Aluminum Ash as Aluminum Correction Raw Material in Clinker Calcination". It also pointed out that "from the perspective of production practice, the addition amount of industrial aluminum ash should not exceed 4.0%, otherwise there will be phenomena such as crusting in the kiln tail smoke chamber and the decomposition furnace cone, thereby affecting the kiln working conditions and bringing disadvantages to production." However, this document also failed to provide an effective solution.

[0005] Therefore, when using recycled aluminum secondary aluminum ash as aluminum correction raw material for silicate cement clinker production, how to achieve its low chlorine and high aluminum content to meet the performance requirements of aluminum correction raw material for silicate cement clinker production, and how to simply treat the secondary aluminum ash on-site harmlessly and without secondary pollution, have become urgent problems to be solved in the resource utilization of secondary aluminum ash. Summary of the invention

[0006] In view of the above reasons, it is necessary to provide a low-chlorine and high-aluminum correction material, production and use based on recycled aluminum secondary aluminum ash, so as to solve the contradiction between the use of secondary aluminum ash as aluminum correction raw material for silicate cement clinker production in the prior art, the amount of secondary aluminum ash added should be as small as possible to ensure that the chloride ion content in the silicate cement clinker does not exceed 0.06%, and the insufficient aluminum content due to the small amount of addition, which further leads to the problem that the performance of the aluminum correction raw material does not meet the requirements. In addition, the production method provided in this application is also expected to be used to solve the problems of energy consumption and unorganized emissions of pollutants such as dust and ammonia caused by multiple operating stations and multiple transfers of materials in the existing aluminum ash harmless treatment methods.

[0007] To achieve the above-mentioned purpose, in the first aspect, the present application provides a method for producing a low-chlorine and high-aluminum correction material based on secondary aluminum ash of recycled aluminum, comprising the steps of using a hydrolysis-washing-filtration integrated tank and performing hydrolysis to remove aluminum nitride and washing and filtering to remove chloride salts in the same hydrolysis-washing-filtration integrated tank, wherein the step of hydrolyzing and removing aluminum nitride is to mix water and the secondary aluminum ash of recycled aluminum in a liquid-solid ratio of (2-10):1 and send them into the hydrolysis-washing-filtration integrated tank, stir and heat to 95°C-100°C to hydrolyze and remove aluminum nitride to obtain hydrolyzed aluminum ash, filtrate and ammonia from which aluminum nitride is removed; and the step of washing and filtering to remove chloride salts uses washing water to wash and filter the hydrolyzed aluminum ash several times to obtain a salt-containing solution and the low-chlorine and high-aluminum correction material.

[0008] The secondary aluminum ash of the recycled aluminum used in the present invention refers to the aluminum ash slag produced from the remelting and refining of waste aluminum, and then the secondary aluminum ash produced after the recovery of metallic aluminum. It is generally the undersize ash produced after the metallic aluminum is extracted by crushing, grinding (commonly known as ball milling), and screening. The average mesh number of the secondary aluminum ash of the recycled aluminum used in the present invention is generally above 150 meshes, so that the low-chloride and high-aluminum correction material obtained after the steps of hydrolysis to remove aluminum nitride and washing and filtering to remove chloride salts can be evenly dispersed in the material when correcting the production of silicate cement raw materials and clay sintered bricks, thereby achieving the effect of improving strength.

[0009] As a further preferred embodiment of the present invention, the method for producing low-chlorine and high-aluminum correction materials further includes an ammonia absorption step, wherein the ammonia absorption step is to absorb the ammonia generated in the hydrolysis and removal of aluminum nitride step with a sulfuric acid solution to generate ammonium sulfate. The ammonium sulfate salt recovered in this step can be further processed and reused as agricultural fertilizer. The ammonia absorption step is carried out in an ammonia absorption tower outside the hydrolysis, washing and filtration integrated tank, and is generally absorbed by spraying.

[0010] As a preferred embodiment of the present invention, the hydrolysis-washing-filtration integrated tank comprises: a tank body, an upper cover arranged on the top of the tank body and a bottom plate arranged on the bottom of the tank body,

[0011] The upper cover is connected to a bracket, an exhaust hole and a feed port, the bracket is fixedly connected to a shaft seat, a rotation drive device and a lifting drive device, a vertically arranged sleeve is rotatably connected in the shaft seat, a lifting shaft that can slide along the axial direction of the sleeve is connected in the sleeve, the lower end of the lifting shaft passes through the upper cover and extends into the tank body, the rotation drive device drives the sleeve to rotate, and the lifting drive device drives the lifting shaft to move up and down along the axial direction of the sleeve, and one end of the lifting shaft located in the tank body is fixedly connected to a stirring blade;

[0012] The bottom plate is provided with a drainage hole connected to the tank body, a filter plate is provided on the upper part of the bottom plate located inside the tank body, a sliding seat adapted to the lower end of the lifting shaft is provided on the bottom plate, a driven shaft is rotatably connected in the sliding seat, the driven shaft is coaxially arranged with the lifting shaft, the filter plate is laid on the upper part of the bottom plate around the sliding seat, the driven shaft extending out of the sliding seat is connected with a scraper rotating with the driven shaft, the scraper is used to scrape out the low-chlorine and high-aluminum correction material on the filter plate;

[0013] A spray device is provided in the inner cavity of the tank body below the feed port, and the spray device is connected to a washing water inlet device; a discharge port is provided on one side of the tank body, and a cover plate is detachably connected to the discharge port; a jacket is provided on the outer wall of the tank body for heating or cooling the material in the tank body, and a filtrate discharge valve is provided at the bottom of the tank body.

[0014] The hydrolysis, washing and filtration integrated tank used in the present invention has a compact structure and composite functions, and can concentrate the stirring, hydrolysis reaction at a specific temperature, washing and filtration required for the treatment of secondary aluminum ash of recycled aluminum in the same hydrolysis, washing and filtration integrated tank. The hydrolysis, washing and filtration integrated tank can be directly set up at the site where the secondary aluminum ash of recycled aluminum needs to be treated and disposed of, and it occupies a small area and is easy to install, so as to achieve "fully enclosed" and "one-stop" treatment of stirring, hydrolysis, washing and filtration of the secondary aluminum ash of recycled aluminum with water, reduce the energy consumption and labor time consumption generated in the material transfer process, and prevent the secondary aluminum ash of recycled aluminum from causing secondary pollution to the environment in the material transfer process of harmless and resource utilization.

[0015] As a further preferred embodiment of the present invention, the ammonia absorption step uses sulfuric acid or a dilute sulfuric acid solution to spray absorb in a first-stage absorption tower and a second-stage absorption tower. Of course, a third-stage absorption tower or even more absorption towers can be further set according to actual conditions to fully eliminate the secondary atmospheric pollution that may be caused by ammonia emissions, and at the same time, achieve the purpose of recovering a larger amount of ammonium sulfate.

[0016] As a further preferred embodiment of the present invention, after the filtration step, the method further includes heating, concentrating and crystallizing the salt solution to obtain an aluminum melting agent (refining agent) for smelting recycled aluminum. In this way, the resource utilization of the secondary aluminum ash of recycled aluminum can be further improved. The aluminum melting agent for smelting recycled aluminum containing chloride salts such as sodium chloride, potassium chloride and magnesium chloride obtained in this step can also be used in other industrial productions that require chloride salts.

[0017] In the second aspect of the present invention, the inventor provides a low-chlorine and high-aluminum correction material based on secondary aluminum ash of recycled aluminum, which is produced by the production method described in the first aspect of the present invention.

[0018] In a further preferred embodiment of the present invention, the chloride ion content of the low-chlorine and high-aluminum correction material is less than or equal to 0.06%, the aluminum nitride content is less than or equal to 1%, and the dry-basis aluminum oxide content is greater than 75%, measured by mass percentage. The low-chlorine and high-aluminum correction material that meets these three indicators is not harmful to the environment and is no longer a hazardous waste listed in the "National Hazardous Waste List". In addition, the sufficiently low chloride ion content and the sufficiently high aluminum oxide content enable it to play the role of aluminum correction raw material in the production of silicate cement clinker.

[0019] In a further preferred embodiment of the present invention, the moisture content of the low-chlorine and high-aluminum correction material is 0%-10%, and can be further dried to achieve the corresponding moisture content requirements according to different application requirements.

[0020] In a third aspect, the present invention provides a use of the low-chlorine high-aluminum correction material described in the second aspect of the present invention as an aluminum correction raw material for the production of Portland cement and clay fired bricks. When used as an aluminum correction raw material for the production of Portland cement, the moisture content of the low-chlorine high-aluminum correction material should be treated to be as small as possible to close to 0; and when used as an aluminum correction raw material for the production of clay fired bricks, the low-chlorine high-aluminum correction material can be kept at a certain moisture content to facilitate transportation and loading and unloading, and to avoid fly ash and dust during transportation and loading and unloading. However, considering the optimal transportation cost and the best use, it is preferred to control its moisture content to 3% to 8%.

[0021] Different from the prior art, the above technical scheme obtains low-chlorine and high-aluminum correction materials by subjecting the secondary aluminum ash raw materials of recycled aluminum to "fully enclosed" and "one-stop" stirring, hydrolysis, washing and filtration in a hydrolysis, washing and filtration integrated tank. Among them, the hydrolysis step reduces the aluminum nitride content to less than 1%, the washing and filtration steps reduce the chloride ion content to less than 0.06%, and the dry basis aluminum oxide content is increased to more than 75%. Further, its moisture content is controlled to 0%-10%, reaching the standard of aluminum correction raw materials for the production of silicate cement and clay sintered bricks, and realizing the harmless treatment and resource utilization of secondary aluminum ash. The production method of the present invention can directly arrange relevant processing equipment on the site where the secondary aluminum ash is generated, and the secondary aluminum ash is harmlessly treated in situ, without unorganized emission pollution of harmful solids and gases such as dust and ammonia, clean and environmentally friendly, and the production method of the present invention has high production efficiency and large production capacity, and the processing facilities have the characteristics of compact overall structure, small space occupation, stable transmission, high reliability and low noise. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A workflow diagram of a method for producing a low-chlorine and high-aluminum correction material based on secondary aluminum ash from recycled aluminum provided in a specific embodiment of the present application;

[0023] Figure 2 Schematic diagram of the production system of low-chlorine and high-aluminum correction material based on recycled aluminum secondary aluminum ash provided in the specific implementation mode of this application.

[0024] Description of reference numerals:

[0025] 1. Tank body; 10. Upper cover; 101. Feed inlet; 102. Bracket; 103. Shaft seat; 104. Rotation drive device; 105. Lifting drive device; 106. Sleeve; 107. Lifting shaft; 108. Stirring blade; 109. Exhaust hole; 110. Spraying device; 111. Drain hole; 112. Filter plate; 113. Scraper; 12. Discharging device; 121. Discharging port. DETAILED DESCRIPTION

[0026] In order to explain the technical content, structural features, achieved objectives and effects of the technical solution in detail, the following is a detailed description in conjunction with specific embodiments and accompanying drawings.

[0027] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.

[0028] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0029] In the description of this application, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in an "or" logical relationship.

[0030] In the present application, terms such as “first” and “second” are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.

[0031] Without further limitations, in this application, the words "include", "comprises", "has" or other similar expressions used in the sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.

[0032] Similar to the understanding in the Examination Guidelines, in this application, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of this application, "multiple" means more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.

[0033] In the description of the embodiments of the present application, space-related expressions used, such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "vertical", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicate the orientation or position relationship based on the orientation or position relationship shown in the specific embodiments or drawings, and are only for the convenience of describing the specific embodiments of the present application or facilitating the reader's understanding, and do not indicate or imply that the referred device or component must have a specific position, a specific orientation, or be constructed or operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0034] Unless otherwise expressly specified or limited, in the description of the embodiments of the present application, the terms such as "install", "connect", "connect", "fix", "set", etc. used should be understood in a broad sense. For example, the "connection" can be a fixed connection, a detachable connection, or an integrated setting; it can be a mechanical connection, an electrical connection, or a communication connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. For technicians in the technical field to which the present application belongs, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0035] "Recycled aluminum secondary aluminum ash" refers to aluminum ash from the recycled aluminum industry. The raw material of the recycled aluminum secondary aluminum ash in the embodiment of the present invention comes from aluminum ash slag produced by remelting and refining waste aluminum, and then secondary aluminum ash produced after recovering metallic aluminum. It is generally the ash under the screen produced after the metallic aluminum is extracted by crushing, grinding (ball milling) and screening. The average mesh size of the recycled aluminum secondary aluminum ash is more than 150 meshes. In this way, the low-chlorine and high-aluminum correction material obtained after the treatment of hydrolysis and filtration can be fully and evenly mixed with other raw materials when correcting the production of silicate cement raw materials and clay bricks to achieve the effect of improving strength.

[0036] "Low chlorine and high aluminum" is the result of long-term investigation, research and practical application of aluminum correction materials used in silicate cement and clay fired bricks. When the chloride ion content in the secondary aluminum ash used as correction material is higher than 0.06%, the secondary aluminum ash is added to the cement raw material to make silicate cement. The chloride ions contained therein will circulate and enrich in the cement kiln system, and continuously cool and volatilize at the kiln tail, causing crusting and blockage; when the amount of secondary aluminum ash added is further increased, the compressive strength of cement continues to decrease, and the chloride ions in cement will cause steel bars in concrete to rust, affecting the life and safety of concrete. When the dry basis aluminum oxide content is lower than 75%, it cannot meet the requirements of silicate cement and clay fired bricks for aluminum content for correction. Therefore, the so-called "low chlorine and high aluminum" in the present invention specifically means that the chloride ion content should be less than or equal to 0.06%, and the aluminum oxide content should be higher than 75%.

[0037] In addition, converting secondary aluminum ash from hazardous waste to general solid waste and reducing the aluminum nitride content to below 1% are basic requirements for the harmless treatment of secondary aluminum ash.

[0038] The detection involved in the present invention is carried out using the methods specified in relevant national standards.

[0039] Example 1

[0040] A low-chlorine high-aluminum correction material based on secondary aluminum ash of recycled aluminum and its production method

[0041] The secondary aluminum ash raw material of the regenerated aluminum in this embodiment comes from the aluminum ash slag produced by the remelting and refining of waste aluminum, and the secondary aluminum ash produced after the recovery of metallic aluminum is generally the ash under the screen produced after the metallic aluminum is extracted by crushing, grinding (ball milling) and screening. The average mesh number of the secondary aluminum ash of the regenerated aluminum is more than 150 meshes. This embodiment uses the same hydrolysis, washing and filtration integrated tank for operation. In other different embodiments, more than one hydrolysis, washing and filtration integrated tank can be set for processing according to the amount of aluminum ash slag to be processed and the actual situation of the site. Clean water and secondary aluminum ash of regenerated aluminum are mixed at a liquid-solid ratio of 3:1 (in other different embodiments, clean water and secondary aluminum ash of regenerated aluminum are mixed at a minimum liquid-solid ratio for easy stirring, or at a liquid-solid ratio of 2-10:1), and are fed into the hydrolysis, washing and filtering integrated tank 1 through the feed port 101 on the upper cover 10, and the lifting drive device 105 installed on the shaft seat 103 installed on the hydrolysis, washing and filtering integrated tank bracket 102 is started to drive the lifting shaft 107 to move upward along the sleeve shaft 106, and the stirring blade 108 in the tank body is raised to the upper part of the filter plate 112 and driven by the rotating drive device 104 to perform the stirring operation. At the same time, the tank jacket is heated to raise the temperature of the mixed system in the tank body to 95°C-100°C for hydrolysis reaction. After stirring and hydrolyzing for 5h-6h, the filtrate discharge valve at the bottom of the tank body is opened to discharge the filtrate into the washing liquid collection pool through the drainage hole 111 on the filter plate 112 on the upper part of the bottom plate. Then, the spray device 110 at the lower part of the feed port is started to wash and filter the harmless regenerated aluminum secondary aluminum ash, i.e., the hydrolyzed aluminum ash, in the hydrolysis, washing and filtration integrated tank for several times. Similarly, the filtrate is discharged into the washing liquid collection pool; until the chloride ion content in the hydrolyzed aluminum ash is less than or equal to 0.06%.

[0042] In other different embodiments, the washing step is to use the previous stage washing water (containing some salt) to wash the hydrolyzed aluminum ash in the next round of hydrolysis, washing and filtration integrated tank to obtain the next stage washing water, that is, the washing water is used in cascade and collected in stages to finally obtain the most concentrated salt solution.

[0043] The ammonia generated in the above stirring and hydrolysis process is fed into the air inlet of the absorption tower through the exhaust hole 109 at the top of the tank body. In the absorption tower, a 1% by mass dilute sulfuric acid solution is used to spray and absorb the ammonia. The (NH 4 ) 2 SO 4 After concentration and crystallization, it can be used to prepare agricultural fertilizer.

[0044] In order to maximize the resource utilization rate of secondary aluminum ash, the salty wastewater produced by multiple washing and desalting can be used as aluminum refining agent and slag-making agent in the secondary aluminum smelting process after evaporation, concentration and crystallization. Of course, it can also be used in other industrial fields that require chloride salts.

[0045] After washing and filtering to discharge the salt-containing wastewater, the rotary drive device 104 is started to drive the scraper 113 to scrape out the residual filter cake on the filter plate 112. The residual filter cake is the low-chlorine and high-aluminum correction material provided by the present invention. According to the measurement, the moisture content of the filter cake is about 8%. The residual filter cake can also be dried according to the user's requirements to make its moisture content lower. If it is to be used in the production of silicate cement, the moisture content is as close to 0 as possible; if it is to be used in the production of clay bricks, the moisture content can be controlled at 3%-8%. Then, the material is discharged from the discharge port 121 through the discharge device 12 to obtain the low-chlorine and high-aluminum correction material.

[0046] After testing, if the low-chloride and high-aluminum correction material meets the requirements of chloride ion content less than 0.06%, aluminum nitride content less than or equal to 1%, aluminum oxide content higher than 75%, and moisture content lower than 10%, it is judged as a qualified product and put into storage.

[0047] If the material discharged from the discharge port is a defective product that does not meet the above indicators, the material discharged from the discharge port will be returned to the hydrolysis, washing and filtration integrated tank for further treatment.

[0048] The low-chlorine high-aluminum correction material and its production method use the simplest treatment facilities and treatment methods to firstly make the rich resources contained in the secondary aluminum ash of recycled aluminum harmless and turn it into general solid waste. Secondly, it maximizes its resource utilization, not only can obtain aluminum correction raw materials for silicate cement production and clay brick production, but also can further obtain ammonium sulfate and chloride salt.

[0049] Example 2

[0050] The low-chlorine high-aluminum correction material obtained in Example 1 is used in the production of silicate cement.

[0051] In order to solve the current situation of decreasing natural high-alumina clay resources, the low-chlorine high-alumina correction material obtained in Example 1 is used to replace natural high-alumina clay and added to cement raw material. The specific method is as follows:

[0052] In terms of mass percentage, the low-chlorine high-aluminum correction material of Example 1 is added to the following cement raw materials in the following proportions for batching: 82% limestone (containing 0.2% alumina), 9% loess (containing 11% alumina), 3% iron powder (containing 2.9% alumina), and 5% low-chlorine high-aluminum correction material (containing 75% alumina). The raw materials are placed in a high-temperature furnace at 1400±50°C for high-temperature calcination to produce clinker. After testing, the quality of the silicate cement clinker meets the requirements of "Silica Cement Clinker GB / T 21372" and "General Purpose Silicate Cement" (GB175).

[0053] The low-chlorine high-aluminum correction material produced based on the secondary aluminum ash of recycled aluminum in this embodiment is used for the raw material batching of silicate cement enterprises, which can reduce the use of natural high-aluminum clay resources, improve the burnability of raw materials, and reduce the coal consumption of the clinker calcining process. It is especially suitable for silicate cement production enterprises with poor limestone grade or high-silicon low-aluminum clay ingredients. According to the relevant provisions of GB / T17671, the test was carried out. After testing, the strength grade of the silicate cement produced by the method of this embodiment is 62.5, which meets the standard strength of GB175 of "General Portland Cement".

[0054] Example 3

[0055] The low-chlorine and high-alumina correction material obtained in Example 1 is used in the production of clay fired bricks.

[0056] In the process of urban development, construction waste and engineering slag have become the main components of urban garbage. Solving the problem of slag treatment and disposal is not only a requirement for beautifying the urban environment, but also directly affects the construction of urban projects. At present, among the various schemes for the resource utilization of slag and construction waste, there is a method of using various types of slag and construction waste to produce sintered bricks. Construction waste such as construction slag, construction mud, waste bricks and tiles are crushed into powder, used as recycled raw materials, and then mixed with clay ingredients to make blanks, and fired into sintered bricks through a brick kiln. Compared with pure clay raw materials without construction waste, excessive mixing of construction slag and waste brick powder has the disadvantages of poor sintering and low strength of fired products. The amount of waste powder is generally limited to less than 5%, which limits the comprehensive recycling of construction waste. Due to the large reduction in landfill land and the depletion of high-quality clay resources year by year, it is imperative to further increase the recycling of construction waste and waste bricks and tiles. Under this circumstance, it is urgent to develop a clay brick production method using the low-chlorine and high-aluminum correction material of the present invention, increasing the mixing ratio of construction waste and waste bricks and tiles, and ensuring the sinterability and strength of the clay bricks after firing. The specific operation steps are as follows:

[0057] First, construction waste such as building debris and waste bricks and tiles are crushed, and then the powder with an average mesh size of more than 150 mesh is screened out. The low-chlorine high-aluminum correction material obtained in Example 1 is added to clay, and the building debris powder: low-chlorine high-aluminum correction material: clay is mixed in a ratio of 40:30:30 to make it uniformly dispersed and formed into a blank, which is sent into a kiln and fired at a sintering temperature of 1200℃±10℃ to form a sintered brick. The bending test shows that its bending failure load is 1694N, compared with the bending failure load of 1396N of the full clay sintered brick. The strength of the fired clay brick obtained by the method of this embodiment is significantly improved, and the use of pure clay raw materials is reduced to 30%, which greatly reduces the production cost of clay sintered bricks.

[0058] Comparative Example 1

[0059] The secondary aluminum ash raw material used in Example 1 is directly used as aluminum correction material for silicate cement production.

[0060] 1. The raw materials of silicate cement are prepared by mixing 82% limestone (containing 0.2% alumina), 12% loess (containing 12% alumina), 3% iron powder (containing 2.9% alumina), and 3% secondary aluminum ash (containing 62.1% alumina and 7.13% chloride ions) which has not been treated by the method of the present invention. The raw materials are placed in a high-temperature furnace at 1400±50℃ for high-temperature calcination to produce clinker. It is found that the production method will cause problems such as ring formation in the kiln and blockage of the kiln tail. The cement clinker produced by this method is tested and found to have a chloride ion content of 0.15%, which exceeds the standard of 0.06% chloride ion in Table 4 of the chemical composition of "General Portland Cement" (GB175-2007).

[0061] Comparative Example 2

[0062] The secondary aluminum ash raw material used in Example 1 is directly used as aluminum correction material for clay sintered brick production.

[0063] First, construction waste such as building debris and waste bricks and tiles are crushed, and then the powder with an average mesh size of more than 150 mesh is screened out, and a low-chlorine high-aluminum correction material is added, mixed with clay, and the building debris powder is mixed with clay at a ratio of 20:80, mixed, and evenly dispersed, formed into a blank, and sent to a kiln, and fired at a sintering temperature of 1200°C to form a sintered brick. According to the bending test, the bending failure load of the sintered brick is 950N, which is much less than the bending failure load of the full clay sintered brick of 1396N, that is, the sintered brick product fired by the comparative example 2 has low strength. At the same time, compared with Example 3, the amount of clay raw material used is 40% more, which also greatly increases the production cost of the sintered brick.

[0064] It should be noted that, although the above embodiments have been described in this article, the patent protection scope of the present invention is not limited thereby. Therefore, based on the innovative concept of the present invention, changes and modifications made to the embodiments described herein, or equivalent structures or equivalent process changes made using the contents of the present invention specification and drawings, directly or indirectly applying the above technical solutions to other related technical fields, are all included in the patent protection scope of the present invention.

Claims

1. A method for producing low-chlorine and high-aluminum correction materials based on secondary aluminum ash of recycled aluminum, characterized in that: The method comprises the steps of using a hydrolysis-washing-filtration integrated tank and performing hydrolysis to remove aluminum nitride, ammonia absorption and washing-filtration to remove chloride salts in the same hydrolysis-washing-filtration integrated tank, wherein: The step of removing aluminum nitride by hydrolysis is to mix water and the secondary aluminum ash of the regenerated aluminum at a liquid-solid ratio of (2-10):1, and send them into the hydrolysis, washing and filtration integrated tank, stir and heat to 95°C-100°C to hydrolyze and remove aluminum nitride, and obtain hydrolyzed aluminum ash, filtrate and ammonia from which aluminum nitride is removed; The step of washing, filtering and removing chloride salts uses washing water to wash and filter the hydrolyzed aluminum ash several times to obtain a salt-containing solution and the low-chloride and high-aluminum correction material; The ammonia absorption step comprises using a sulfuric acid solution to absorb the ammonia generated in the step of hydrolyzing and removing aluminum nitride to generate ammonium sulfate; The hydrolysis-washing-filtration integrated tank comprises: a tank body, an upper cover arranged on the top of the tank body and a bottom plate arranged on the bottom of the tank body. The upper cover is connected to a bracket, an exhaust hole and a feed port, the bracket is fixedly connected to a shaft seat, a rotation drive device and a lifting drive device, a vertically arranged sleeve is rotatably connected in the shaft seat, a lifting shaft that can slide along the axial direction of the sleeve is connected in the sleeve, the lower end of the lifting shaft passes through the upper cover and extends into the tank body, the rotation drive device drives the sleeve to rotate, and the lifting drive device drives the lifting shaft to move up and down along the axial direction of the sleeve, and one end of the lifting shaft located in the tank body is fixedly connected to a stirring blade; The bottom plate is provided with a drainage hole connected to the tank body, a filter plate is provided on the upper part of the bottom plate located inside the tank body, a sliding seat adapted to the lower end of the lifting shaft is provided on the bottom plate, a driven shaft is rotatably connected in the sliding seat, the driven shaft is coaxially arranged with the lifting shaft, the filter plate is laid on the upper part of the bottom plate around the sliding seat, the driven shaft extending out of the sliding seat is connected with a scraper rotating with the driven shaft, the scraper is used to scrape out the low-chlorine and high-aluminum correction material on the filter plate; A spray device is provided in the inner cavity of the tank body below the feed port, and the spray device is connected to a washing water inlet device; a discharge port is provided on one side of the tank body, and a cover plate is detachably connected to the discharge port; a jacket is provided on the outer wall of the tank body for heating or cooling the material in the tank body, and a filtrate discharge valve is provided at the bottom of the tank body.

2. The production method according to claim 1, characterized in that The exhaust hole is connected with the air inlet of the ammonia absorption tower.

3. The production method according to claim 1, characterized in that After the washing, filtering and chloride salt removal step, the method further includes heating, concentrating and crystallizing the salt solution to obtain an aluminum melting agent for regenerated aluminum smelting.

4. A low-chlorine and high-aluminum correction material based on secondary aluminum ash of recycled aluminum, characterized in that: The method is produced according to any one of claims 1 to 3.

5. The low-chlorine and high-aluminum correction material according to claim 4, characterized in that: Calculated by mass percentage of the low-chlorine and high-aluminum correction material, the chloride ion content is less than 0.06%, the aluminum nitride content is less than or equal to 1%, and the dry-basis aluminum oxide content is greater than 75%.

6. The low-chlorine and high-aluminum correction material according to claim 5, characterized in that: The water content of the low-chlorine and high-aluminum correction material is 0%-10%.

7. Use of the low-chlorine and high-alumina correction material according to claim 5 as an aluminum correction raw material for the production of silicate cement or clay fired bricks.

8. The use according to claim 7, characterized in that When the low-chlorine and high-aluminum correction material is used as an aluminum correction raw material for the production of silicate cement, the moisture content of the low-chlorine and high-aluminum correction material is controlled to be close to 0%; when the low-chlorine and high-aluminum correction material is used as an aluminum correction raw material for the production of clay sintered bricks, the moisture content of the low-chlorine and high-aluminum correction material is controlled to be 3%-8%.

Citation Information

Patent Citations

  • Methods of using aluminum ash as fuel, corrective agent and calcination aid in dry process cement production

    CN114524630B

  • Method for comprehensively recycling mixed secondary aluminum dross

    CN109678180A