Highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film and preparation method and use thereof
Through the preparation of highly flame retardant carboxylated sisal fiber nanocrystalline/graphene composite film, the shortcomings of existing materials in flame retardant performance and fire early warning sensing are solved, and the combination of high flame retardant and multifunctional performance is achieved. , provides green and sustainable solutions.
Patent Information
- Application Number
- CN202310275733.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-21
AI Technical Summary
The existing polymer film materials have shortcomings in flame retardant performance and fire early warning sensing functions, which cannot meet the needs of green environmental protection, high flame retardant and multifunctional performance. The addition of traditional flame retardant will affect the mechanical properties of the material and Production cost.
The preparation method of highly flame retardant carboxylated sisal fiber nanocrystalline/graphene composite film is adopted, and carboxymethyl chitosan and phytic acid are used in ferric chloride solution. It is evenly dispersed to form a highly flame retardant composite film, and improves its flame retardant performance and sensing function through the immersion and drying process.
Achieve high flame retardant performance, the flame retardant test results reach 37% limit oxygen index and V-0 level vertical combustion level, and have temperature and flame sensing functions, suitable for fire alarm and temperature measurement sensors, and the material is green continued.
Smart Images

Figure CN116376088B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film and a preparation method and application thereof. Background Art
[0002] With the development of the times and the improvement of environmental protection requirements, polymer film materials are widely used in various fields such as agriculture, national defense, construction, and electronic industry, and the requirements for the safety and green sustainable development of the materials themselves are becoming higher and higher. Traditional polymer-based (such as polypropylene, polyethylene, etc.) films have good mechanical properties, but the matrix materials are non-renewable, have poor flame retardancy, and have single functions, which cannot meet the multifunctional performance requirements of green environmental protection, high flame retardancy, etc. proposed in some special fields. Sisal cellulose nanocrystals are abundant in sources and are green and renewable nanomaterials. They have the advantages of low cost, large aspect ratio, large specific surface area, high flexibility, and good biocompatibility. The mechanical properties of the nanocomposite film materials made from them are much higher than those of conventional film materials, but the flame retardancy is poor. At present, the common method to improve the flame retardancy is to add flame retardants to polymer materials, such as hydroxides (such as Mg(OH)2) and phosphorus-nitrogen flame retardants (such as ammonium polyphosphate, etc.), but a higher addition amount may cause the loss of mechanical properties of the film material and increase the production cost. Chinese patent CN201811198628.1 introduces a graphene-based flame-retardant and heat-resistant sisal cellulose film. A flame-retardant and heat-resistant sisal cellulose film is prepared using pentaerythritol, phosphorus oxychloride, melamine, graphene, etc. as raw materials, but the preparation process is complicated and does not involve the multifunctional requirements of sensing.
[0003] In the face of the increasingly severe fire safety prevention situation, in addition to improving the flame retardant properties of materials, sensitive fire warning systems can also be used to eliminate hidden dangers from the source as much as possible and reduce the occurrence of fire accidents. Among them, fire warning sensors are the key to reducing the incidence of fire and fire losses. Existing fire warning devices are mainly smoke alarms and infrared alarms, each with its own shortcomings. They are often installed on the top of the ceiling or wall of the building. Usually, the alarm can only be triggered when the smoke concentration or thermal infrared intensity exceeds a certain value, and the response time is often long. Therefore, it is urgent to design a new type of fire warning sensor.
[0004] Therefore, how to use a simple and effective preparation method to prepare a green, environmentally friendly, highly flame-retardant bio-based composite film with fire warning sensing function and improve the sensitivity of fire warning sensing is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film. Another object of the present invention is to provide a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film. Another object of the present invention is to provide a use of a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] The method for preparing a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film comprises the following steps performed in sequence:
[0008] 1) uniformly dispersing carboxylated sisal fiber nanocrystals in water or hydrochloric acid aqueous solution, then adding carboxymethyl chitosan and graphene, and mixing them uniformly to form a precursor solution;
[0009] 2) preparing the precursor solution into a thin film to obtain a composite thin film;
[0010] 3) The prepared composite film is sequentially immersed in a ferric chloride solution and a phytic acid solution, and then dried to obtain a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film.
[0011] Preferably, the carboxylated sisal fiber nanocrystals have a length of 150 to 200 nm and a diameter of 2 to 6 nm.
[0012] Preferably, the molecular weight of the carboxymethyl chitosan is 200-240Kda, the degree of deacetylation is 75%-95%, and the degree of substitution is 85%-92%.
[0013] Preferably, the graphene has a monolayer ratio of >90%, a thickness of 0.6-1.2 nm, and a sheet diameter of 1-5 μm.
[0014] Preferably, the mass of carboxylated sisal fiber nanocrystals: the mass of carboxymethyl chitosan: the mass of graphene = (70-100): (10-25): (1-15).
[0015] Preferably, the preparation method of carboxylated sisal fiber nanocrystals in step 1) is:
[0016] 1.1) mixing sisal fiber, organic acid, sodium chlorite and water at 80° C. to 90° C., and then washing the obtained product with water;
[0017] 1.2) taking the sisal fiber treated in step 1.1), alkali, chloroacetic acid and ethanol, stirring and mixing at 80° C. to 90° C., and then washing the obtained product with water until the obtained product is neutral;
[0018] 1.3) After high-speed shearing at 25000-30000 r / min, carboxylated sisal fiber nanocrystals having a transparent gel state are obtained.
[0019] Preferably, the organic acid is one or a combination of acetic acid, glycolic acid, citric acid, and aminosulfonic acid;
[0020] The alkali is one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, sodium bicarbonate or a combination thereof.
[0021] A highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film prepared by the method for preparing a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film as described in any one of the above.
[0022] A highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film prepared by the preparation method of any one of the above-mentioned highly flame retardant carboxylated sisal fiber nanocrystals / graphene composite films or the highly flame retardant carboxylated sisal fiber nanocrystals / graphene composite film is used as a temperature switch in a fire alarm.
[0023] A highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film prepared by the method for preparing a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film as described in any one of the above or the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film as a temperature sensor.
[0024] Compared with the prior art, the present invention provides a method for preparing a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film, which has the following excellent technical effects: the composite film has excellent flame retardant properties, the result of the flame retardant test can reach a limiting oxygen index of 37%, and the vertical combustion UL-94 test grade reaches V-0 level;
[0025] The composite film has the function of a sensor, and can perform temperature sensing and flame sensing. Tests have shown that the composite film can be used as a temperature switch in a fire alarm, and can also be used as a temperature sensor.
[0026] The composite film is a green and sustainable bio-based material. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. It is obvious that the following drawings are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0028] Figure 1 This is a surface SEM image of the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film prepared in Example 3;
[0029] Figure 2 This is the thermal temperature sensing current response diagram of the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film synthesized in Example 3. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings and attached tables in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of them. Therefore, based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present invention provides a method for preparing a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film, which specifically comprises the following steps performed in sequence:
[0032] 1) Add 70-85 parts of carboxylated sisal fiber nanocrystals into a glass container, then add 100-200 parts of deionized water or hydrochloric acid aqueous solution, and mix to form a uniform solution;
[0033] 2) adding 15 to 25 parts of carboxymethyl chitosan into a glass container, then adding 50 to 80 parts of deionized water, heating to 40 to 80° C. under stirring to form a uniform solution;
[0034] 3) adding 5 to 15 parts of graphene into a glass container, then adding 40 to 80 parts of deionized water, and heating to 40 to 80° C. under stirring to form a uniform solution;
[0035] 4) adding 0.1 to 1.5 parts of ferric chloride into a glass container, and then adding 100 to 200 parts of deionized water, and mixing to form a uniform solution;
[0036] 5) adding 1-2 parts of phytic acid into a glass container, and then adding 100-200 parts of deionized water, and mixing to form a uniform solution;
[0037] 6) adding the solution obtained in step 2) to the carboxylated sisal fiber nanocrystal solution in step 1) and stirring evenly, heating to 40-80° C. under stirring conditions and reacting for 0.5-1.5 hours to obtain a mixed solution of evenly dispersed carboxylated sisal fiber nanocrystals and carboxymethyl chitosan;
[0038] 7) adding the graphene solution obtained in step 3) to the solution obtained in step 6) at 40-80° C., then reacting at 60-80° C. for 1-4 hours, adding 0.5%-2wt% of glycerol and continuing stirring for 0.2-1 hour to obtain a precursor solution;
[0039] 8) subjecting the obtained precursor solution to ultrasonic dispersion treatment, pouring it into a mold, placing it in a vacuum oven at 60-80° C. for 12-24 hours, and preparing a composite film by a vacuum casting film forming method;
[0040] 9) The composite film is sequentially immersed in the solution obtained in step 4) and step 5) for 3 to 10 minutes each, and then dried at 60° C. to 80° C. for 2 to 8 hours to obtain a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film.
[0041] In the present application, the concentration of the aqueous hydrochloric acid solution (aqueous solution of hydrogen chloride) is 0.04-0.08 mol / L.
[0042] In the present invention, the preparation method of carboxylated sisal fiber nanocrystals is specifically as follows:
[0043] 1) 200-500 g of sisal fiber, 8-20 ml of acetic acid, 8-20 g of sodium chlorite and 500-800 ml of deionized water are stirred in a three-necked flask at 80° C.-90° C. for 2-5 hours, and then the obtained product is washed three times with deionized water;
[0044] 2) taking 200-500 g of the sisal fiber treated in step 1), 2-5 g of sodium hydroxide, 5-15 g of chloroacetic acid and 150-300 ml of ethanol and stirring at 80° C.-90° C. for 2-3 hours, and washing the obtained product with deionized water until it becomes neutral;
[0045] 3) high-speed shearing at 25000-30000 r / min for 0.5-1.5 hours, and after completion, carboxylated sisal fiber nanocrystals in the shape of a transparent gel are obtained.
[0046] In the present application, the mass of carboxylated sisal fiber nanocrystals: the mass of carboxymethyl chitosan: the mass of graphene = (70-100): (10-25): (1-15), preferably (70-85): (15-25): (5-15), and further preferably (70-78): (15-20): (8-12).
[0047] Functions and effects of each raw material in the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film of the present application:
[0048] Functions and effects of carboxylated sisal fiber nanocrystals: As a matrix material, it provides structural support for the film and gives the film material basic flexibility, foldability and mechanical properties;
[0049] Functions and effects of carboxymethyl chitosan: On the one hand, carboxymethyl chitosan enhances the interrelationship between material matrices, which helps to improve the stability of the material network structure; on the other hand, the excellent water solubility and film-forming properties of carboxymethyl chitosan further simplify the preparation process of composite films. In addition, the combination of carboxymethyl chitosan and phytic acid has a good synergistic flame retardant effect, giving the film material high flame retardant properties;
[0050] Functions and effects of graphene: With the help of graphene's excellent thermal and electrical conductivity, the film material is endowed with sensing properties, and it serves as a skeleton to support the overall structure of the burning object during the combustion process; the introduction of graphene can enhance the flame retardant and mechanical properties of the composite film (nano-enhanced effect), while also giving the film material good temperature sensing properties;
[0051] Functions and effects of ferric chloride solution: The trivalent iron ions in ferric chloride can act as a cross-linking agent, chelated by the matrix material and phytic acid, and fix the phytic acid molecules by chemical bonds; the iron ions as a cross-linking agent can effectively combine the introduced phytic acid with the composite film, thereby improving the flame retardant properties of the film material;
[0052] Functions and effects of phytic acid: As a natural substance with high phosphorus content, phytic acid is used as a phosphorus flame retardant in materials, and works synergistically with carboxymethyl chitosan to achieve high flame retardancy;
[0053] The interaction between these raw materials enables the composite film prepared by the present invention to have excellent properties in terms of flame retardancy, sensing, acid and alkali resistance, etc.
[0054] The reason or working principle of the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film of the present application having high flame retardancy is as follows: when the composite film is attacked by external flames, the phytic acid decomposition promotes the dehydration of the macromolecular matrix to form a stable carbon layer. At the same time, the macromolecular matrix containing nitrogen elements releases non-flammable gas during the combustion process, which promotes the expansion of the carbon layer and effectively dilutes the oxygen concentration on the surface of the material, further inhibiting combustion.
[0055] The working principle of the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film having sensor function in this application is as follows:
[0056] (1) The temperature sensitivity of the composite film is due to the fact that the increase in temperature promotes the movement of carriers between graphene sheets, thereby reducing the overall resistance of the material. When an external circuit is connected, the current change can be clearly observed, thereby achieving temperature sensing;
[0057] (2) The flame sensitivity of the composite film is due to the fact that the graphene is initially coated in a non-conductive polymer matrix. The film material exhibits a large resistance value in the circuit and cannot effectively connect the circuit as a conductor. After contact with the flame, a dense carbon layer is formed on the surface of the film material, the graphene network is connected, and the conductivity is significantly increased, thereby achieving flame sensing.
[0058] The highly flame retardant carboxylated sisal fiber nanocrystals / graphene composite film of the present application has the working principle of green and sustainable bio-based materials: the raw materials of the composite film are all natural materials, the raw materials of carboxylated sisal fiber nanocrystals come from sisal, the raw materials of carboxymethyl chitosan are widely distributed in crustaceans, and phytic acid also comes from nuts. From the perspective of raw materials, the film material is a green and sustainable bio-based material.
[0059] The working principle of the method for preparing carboxylated sisal fiber nanocrystals of the present application is as follows:
[0060] The sisal fiber is grafted and modified by chemical reaction, so that a large number of carboxyl groups are present on its surface. The water solubility of natural cellulose materials is poor and they cannot be effectively dispersed in aqueous solution. The modified carboxylated sisal fiber nanocrystals carry hydrophilic carboxyl groups, which effectively improves the solubility of sisal fiber in water, and the solution can remain stable and uniform for a long time.
[0061] The carboxylation treatment of sisal fiber is green, environmentally friendly, simple and easy to implement with high yield; at the same time, the carboxylation of sisal fiber nanocrystals improves the dispersibility of sisal fiber in water, and can react with hydrophilic functional groups such as amino and hydroxyl groups on the surface of carboxymethyl chitosan, which helps to improve the stability and mechanical properties of the composite film.
[0062] In the present application, the water dispersibility of sisal fiber is improved by carboxylation; the nano-enhancement effect of graphene and the active functional groups (amino and hydroxyl groups) of carboxymethyl chitosan can simultaneously improve the overall stability and flame retardant properties of the composite film. Carboxymethyl chitosan can not only form hydrogen bonds with carboxylated sisal fiber nanocrystals to bridge the nanofiber network, but also synergize with phytic acid to exert a flame retardant effect. Moreover, the introduction of graphene also gives the composite film excellent temperature sensitivity, which is suitable for the field of flame retardant protective layers and fire alarm sensors.
[0063] The methods and devices not described in detail in the present invention are all prior art and will not be described in detail.
[0064] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0065] The raw materials of the invention are conventional products on the market, and the specific preparation operation and testing are conventional technologies; the molecular weight of the used carboxymethyl chitosan is 200-240Kda, the deacetylation degree is 75%-95%, and the substitution degree is 85%-92%.
[0066] Example 1
[0067] 1) Preparation of carboxylated sisal fiber nanocrystals: 200 g sisal fiber, 8 ml acetic acid, 8 g sodium chlorite and 600 ml deionized water were stirred in a three-necked flask at 80° C. for 2 hours, and then the obtained product was washed three times with deionized water;
[0068] Then, 200 g of the treated sisal fiber, 2 g of sodium hydroxide, 5 g of chloroacetic acid and 300 ml of ethanol were stirred at 80 °C for 2 hours, and the obtained product was washed with deionized water until it was neutral;
[0069] Then, the fiber was sheared at 25000 r / min for 0.5 hours, and carboxylated sisal fiber nanocrystals were obtained.
[0070] 2) adding 40 g of carboxylated sisal fiber nanocrystals into a glass container at room temperature, and then adding 50 g of hydrochloric acid aqueous solution, and mixing to form a uniform solution;
[0071] Since the surface of carboxylated sisal fiber nanocrystals contains a large number of hydrophilic groups, they show good solubility in aqueous solution and weak acid solution, and a uniformly dispersed system is obtained;
[0072] 3) adding 7.5 g of carboxymethyl chitosan into a glass container at room temperature, then adding 35 g of deionized water, and then heating to 45° C. under stirring to form a uniform solution;
[0073] 4) adding 2.5 g of graphene into a glass container at room temperature, then adding 35 g of deionized water, and then heating to 60° C. under stirring to form a uniform solution;
[0074] 5) Add 0.05 g of ferric chloride into a glass container at room temperature, then add 100 g of deionized water and mix to form a uniform solution;
[0075] 6) adding 0.5 g of phytic acid into a glass container at room temperature, and then adding 100 g of deionized water, and mixing to form a uniform solution;
[0076] 7) at room temperature, adding the solution obtained in step 3) to the carboxylated sisal fiber nanocrystal solution in step 2) and stirring evenly, heating to 80° C. under stirring for 1.5 hours to obtain a mixed solution of evenly dispersed carboxylated sisal fiber nanocrystals and carboxymethyl chitosan;
[0077] 8) adding the graphene solution obtained in step 4) to the solution obtained in step 7) at 80° C., reacting at 80° C. for 1 hour, adding 0.1 g of glycerol and continuing stirring for 0.2 hours to obtain a precursor solution;
[0078] 9) subjecting the obtained precursor solution to ultrasonic dispersion treatment, then pouring it into a mold, and then placing it in a vacuum oven at 60° C. for 24 hours, and preparing a composite film by a vacuum casting film forming method;
[0079] 10) The composite film is sequentially immersed in the solutions obtained in step 5) and step 6) for 3 minutes each, and then dried at 80° C. for 4 hours to finally prepare a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film.
[0080] Example 2
[0081] 1) Preparation of carboxylated sisal fiber nanocrystals: 250 g sisal fiber, 15 ml acetic acid, 15 g sodium chlorite and 600 ml deionized water were stirred in a three-necked flask at 85° C. for 2.5 hours, and the obtained product was washed three times with deionized water;
[0082] Then, 200 g of the treated sisal fiber, 2.5 g of sodium hydroxide, 10 g of chloroacetic acid and 250 ml of ethanol were stirred at 85 °C for 2 hours, and the obtained product was washed with deionized water until it was neutral;
[0083] Then, the fiber was sheared at a high speed of 30,000 r / min for 1 hour, and carboxylated sisal fiber nanocrystals were obtained.
[0084] 2) adding 40 g of carboxylated sisal fiber nanocrystals into a glass container at room temperature, and then adding 80 g of deionized water, and mixing to form a uniform solution;
[0085] Since the surface of carboxylated sisal fiber nanocrystals contains a large number of hydrophilic groups, they show good solubility in aqueous solution and weak acid solution, and a uniformly dispersed system is obtained;
[0086] 3) adding 10 g of carboxymethyl chitosan into a glass container at room temperature, then adding 40 g of deionized water, and then heating to 45° C. under stirring to form a uniform solution;
[0087] 4) adding 2.5 g of graphene into a glass container at room temperature, then adding 40 g of deionized water, and then heating to 40° C. under stirring to form a uniform solution;
[0088] 5) Add 0.05 g of ferric chloride into a glass container at room temperature, then add 100 g of deionized water and mix to form a uniform solution;
[0089] 6) adding 0.5 g of phytic acid into a glass container at room temperature, and then adding 100 g of deionized water, and mixing to form a uniform solution;
[0090] 7) at room temperature, adding the solution obtained in step 3) to the carboxylated sisal fiber nanocrystal solution in step 2) and stirring evenly, heating to 60° C. under stirring for 1 hour to obtain a mixed solution of evenly dispersed carboxylated sisal fiber nanocrystals and carboxymethyl chitosan;
[0091] 8) adding the graphene solution obtained in step 4) to the solution obtained in step 7) at 60° C., and then reacting at 80° C. for 1 hour, adding 0.15 g of glycerol and continuing stirring for 0.5 hour to obtain a precursor solution;
[0092] 9) subjecting the obtained precursor solution to ultrasonic dispersion treatment, then pouring it into a mold, and then placing it in a vacuum oven at 80° C. for 20 hours, and preparing a composite film by a vacuum casting film forming method;
[0093] 10) The composite film is sequentially immersed in the solutions obtained in step 5) and step 6) for 10 minutes each, and then dried at 70° C. for 3 hours to finally prepare the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film.
[0094] Example 3
[0095] 1) Preparation of carboxylated sisal fiber nanocrystals: 250 g sisal fiber, 10 ml acetic acid, 10 g sodium chlorite and 500 ml deionized water were stirred at 90° C. for 3 hours in a three-necked flask, and the obtained product was washed three times with deionized water;
[0096] Then, 230 g of the treated sisal fiber, 2 g of sodium hydroxide, 5 g of chloroacetic acid and 150 ml of ethanol were stirred at 90 °C for 2 hours, and the obtained product was washed with deionized water until it was neutral;
[0097] Then, the fiber was sheared at 25000 r / min for 1 hour, and carboxylated sisal fiber nanocrystals were obtained.
[0098] 2) adding 40 g of carboxylated sisal fiber nanocrystals into a glass container at room temperature, and then adding 60 g of deionized water, and mixing to form a uniform solution;
[0099] Since the surface of carboxylated sisal fiber nanocrystals contains a large number of hydrophilic groups, they show good solubility in aqueous solution and weak acid solution, and a uniformly dispersed system is obtained;
[0100] 3) adding 10 g of carboxymethyl chitosan into a glass container at room temperature, then adding 30 g of deionized water, and then heating to 50° C. under stirring to form a uniform solution;
[0101] 4) adding 4 g of graphene into a glass container at room temperature, then adding 40 g of deionized water, and then heating to 70° C. under stirring to form a uniform solution;
[0102] 5) Add 0.05 g of ferric chloride into a glass container at room temperature, then add 100 g of deionized water and mix to form a uniform solution;
[0103] 6) Add 1 g of phytic acid into a glass container at room temperature, then add 100 g of deionized water, and mix to form a uniform solution;
[0104] 7) at room temperature, adding the solution obtained in step 3) to the carboxylated sisal fiber nanocrystal solution in step 2) and stirring evenly, heating to 70° C. for reaction for 1 hour under stirring conditions to obtain a mixed solution of evenly dispersed carboxylated sisal fiber nanocrystals and carboxymethyl chitosan;
[0105] 8) adding the graphene solution obtained in step 4) to the solution obtained in step 7) at 70° C., and then reacting at 80° C. for 2 hours, adding 0.1 g of glycerol and continuing to stir for 0.5 hours to obtain a precursor solution;
[0106] 9) subjecting the obtained precursor solution to ultrasonic dispersion treatment, then pouring it into a mold, and then placing it in a vacuum oven at 80° C. for 12 hours, and preparing a composite film by a vacuum casting film forming method;
[0107] 10) The composite film is sequentially immersed in the solutions obtained in step 5) and step 6) for 5 minutes each, and then dried at 60° C. for 3 hours to finally prepare the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film.
[0108] Comparative Example 1
[0109] 1) preparing carboxylated sisal fiber nanocrystals according to the method of Example 3;
[0110] 2) adding 40 g of carboxylated sisal fiber nanocrystals into a glass container at room temperature, and then adding 60 g of deionized water, and mixing to form a uniform solution;
[0111] Since the surface of carboxylated sisal fiber nanocrystals contains a large number of hydrophilic groups, they show good solubility in aqueous solution and weak acid solution, and a uniformly dispersed system is obtained;
[0112] 3) adding 10 g of carboxymethyl chitosan into a glass container at room temperature, then adding 30 g of deionized water, and then heating to 50° C. under stirring to form a uniform solution;
[0113] 4) adding the solution obtained in step 3) to the carboxylated sisal fiber nanocrystal solution in step 2) at room temperature and stirring evenly, heating to 70° C. for reaction for 1 hour under stirring to obtain a uniformly dispersed precursor solution of carboxylated sisal fiber nanocrystals and carboxymethyl chitosan;
[0114] 5) The obtained precursor solution is subjected to ultrasonic dispersion treatment, then poured into a mold, and then placed in a vacuum oven for treatment at 80° C. for 12 hours, and a composite thin film material is prepared by a vacuum casting film forming method.
[0115] Comparative Example 2
[0116] 1) preparing carboxylated sisal fiber nanocrystals according to the method of Example 3;
[0117] 2) adding 40 g of carboxylated sisal fiber nanocrystals into a glass container at room temperature, and then adding 60 g of deionized water, and mixing to form a uniform solution;
[0118] Since the surface of carboxylated sisal fiber nanocrystals contains a large number of hydrophilic groups, they show good solubility in aqueous solution and weak acid solution, and a uniformly dispersed system is obtained;
[0119] 3) adding 10 g of carboxymethyl chitosan into a glass container at room temperature, then adding 30 g of deionized water, and then heating to 50° C. under stirring to form a uniform solution;
[0120] 4) adding 4 g of graphene into a glass container at room temperature, then adding 40 g of deionized water, and then heating to 70° C. under stirring to form a uniform solution;
[0121] 5) adding the solution obtained in step 3) to the carboxylated sisal fiber nanocrystal solution in step 2) at room temperature and stirring evenly, heating to 70° C. for reaction for 1 hour under stirring to obtain a mixed solution of evenly dispersed carboxylated sisal fiber nanocrystals and carboxymethyl chitosan;
[0122] 6) adding the graphene solution obtained in step 4) to the solution obtained in step 7) at 70° C., and then reacting at 80° C. for 2 hours, adding 0.1 g of glycerol and continuing to stir for 0.5 hours to obtain a precursor solution;
[0123] 7) The obtained precursor solution is subjected to ultrasonic dispersion treatment, then poured into a mold, and then placed in a vacuum oven for treatment at 80° C. for 12 hours, and a composite thin film material is prepared by a vacuum casting film forming method.
[0124] The test showed that the composite film prepared in Example 3 could be rolled and folded without any mechanical damage and the surface remained smooth, indicating that the highly flame-retardant composite film provided by the present invention had excellent flexibility and deformation ability.
[0125] In addition, from Figure 1 From the SEM image, the microscopic surface of the film material prepared in Example 3 has a rough structure, which proves that ferric chloride and phytic acid are successfully attached to the surface of the material, thereby improving the flame retardant properties of the composite film.
[0126] It can be obtained through experiments that the composite film prepared in Example 3 and other circuit elements form a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film fire alarm system; a simple fire alarm system is prepared by connecting a battery, an alarm, and the composite film prepared in Example 3 to form a circuit; when not in contact with the flame, the circuit is disconnected and the alarm cannot be triggered; when the composite film contacts the flame, the circuit is connected, the alarm is triggered, and a sound and light prompt are emitted;
[0127] This is because the graphene in the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film was initially coated in a non-conductive polymer matrix. The film material exhibited a large resistance value in the circuit and could not effectively connect the circuit as a conductor. After contact with the flame, a dense carbon layer was formed on the surface of the film material, and the graphene network was connected, and the conductivity was significantly increased. When the circuit was connected, the alarm was triggered, thereby achieving flame sensing, indicating that the film material has application value in fire alarm sensors.
[0128] Figure 2 The thermal temperature sensing current response of the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film synthesized in Example 3; when the composite film prepared in Example 3 is placed at different temperatures (60°C to 200°C), the circuit shows different degrees of current response, and the initial current value can be restored after the temperature is lowered, and the current response is still stable after repeated heating-cooling, indicating that the film material has sensitive, stable and reversible temperature sensing capabilities;
[0129] The temperature sensitivity of the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film is due to the fact that the increase in temperature promotes the movement of carriers between graphene sheets, thereby reducing the overall resistance of the material. In the case of an external circuit, the current change can be clearly observed, thereby achieving temperature sensing, indicating that the film material has application value in the field of temperature sensors.
[0130] Table 1 Flame retardant performance test results of the embodiments and comparative examples
[0131] Limiting oxygen index (%) Vertical burning grade UL-94 Comparative Example 1 22 No level Comparative Example 2 26 No level Example 3 37 V-0
[0132] As can be seen from Table 1, after adding phytic acid for flame retardancy, the flame retardant performance of the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film prepared in Example 3 is much higher than that of Comparative Example 1 and Comparative Example 2, the limiting oxygen index reaches 37%, and the vertical combustion grade is VO, that is, the material is self-extinguishing when away from the fire and will not melt and drip. The limiting oxygen index and vertical combustion grade in Table 1 meet the requirements of flame retardant materials, confirming the high flame retardancy of the film material;
[0133] When the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film is attacked by external flames, the phytic acid decomposition promotes the dehydration of the macromolecular matrix to form a stable carbon layer. At the same time, the nitrogen-containing macromolecular matrix releases non-flammable gas during the combustion process, which promotes the expansion of the carbon layer and effectively dilutes the oxygen concentration on the surface of the material, further inhibiting combustion. The above-mentioned multiple effects together create the high flame retardant performance of Example 3.
[0134] The above results show that the product of the present invention has potential practical application prospects as a highly flame-retardant composite thin film sensor. The product of the present invention can be a thin film, which can be used directly or in combination to obtain a multifunctional product with richer functions.
[0135] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film, characterized in that: The method includes the following steps: 1) Dispersing carboxylated sisal fiber nanocrystals uniformly in water or hydrochloric acid aqueous solution, then adding carboxymethyl chitosan and graphene, and mixing uniformly to form a precursor solution; 2) preparing the precursor solution into a thin film to obtain a composite thin film; 3) soaking the prepared composite film in a ferric chloride solution and a phytic acid solution in turn, and then drying, to obtain a highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film; The mass of carboxylated sisal fiber nanocrystals: the mass of carboxymethyl chitosan: the mass of graphene = (70~100): (10~25): (1~15).
2. The method for preparing the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film according to claim 1, characterized in that: The length of the carboxylated sisal fiber nanocrystals is 150-200 nm and the diameter is 2-6 nm.
3. The method for preparing the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film according to claim 1, characterized in that: The molecular weight of the carboxymethyl chitosan is 200-240 KDa, the deacetylation degree is 75%-95%, and the substitution degree is 85%-92%.
4. The method for preparing the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film according to claim 1, characterized in that: The monolayer rate of graphene is >90%, the thickness is 0.6-1.2nm, and the sheet diameter is 1-5μm.
5. The method for preparing the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film according to claim 1, characterized in that: The preparation method of carboxylated sisal fiber nanocrystals in step 1) is: 1.1) Mixing sisal fiber, organic acid, sodium chlorite and water at 80°C to 90°C, and then washing the obtained product with water; 1.2) taking the sisal fiber treated in step 1.1), alkali, chloroacetic acid and ethanol, stirring and mixing at 80° C. to 90° C., and then washing the obtained product with water until the obtained product is neutral; 1.3) After high-speed shearing at 25000-30000 r / min, carboxylated sisal fiber nanocrystals with transparent gelatinous state are obtained.
6. The method for preparing the highly flame-retardant carboxylated sisal fiber nanocrystal / graphene composite film according to claim 5, characterized in that: The organic acid is one of acetic acid, glycolic acid, citric acid, and aminosulfonic acid, or a combination thereof; The alkali is one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, sodium bicarbonate or a combination thereof.
7. A highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film prepared by the method for preparing a highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film according to any one of claims 1 to 6.
8. Use of the highly flame retardant carboxylated sisal fiber nanocrystals / graphene composite film prepared by the preparation method of the highly flame retardant carboxylated sisal fiber nanocrystals / graphene composite film according to any one of claims 1 to 6 or the highly flame retardant carboxylated sisal fiber nanocrystals / graphene composite film according to claim 7 as a temperature switch in a fire alarm.
9. Use of the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film prepared by the preparation method of the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film according to any one of claims 1 to 6 or the highly flame retardant carboxylated sisal fiber nanocrystal / graphene composite film according to claim 7 as a temperature sensor.