Unzipping carbon nanotubes carrying transition metal-reinforced nylon 66 and method thereof

By using unzipped carbon nanotubes carrying transition metal reinforcement technology in nylon 66, the problems of low strength of nylon 66 and uneven distribution of carbon nanotubes were solved, which significantly improved the mechanical properties of the material, and achieved the strength of nylon 66 material and Modulus increases.

CN116376275BActive Publication Date: 2024-11-22QINGDAO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310433023.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-11-22
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

The low strength of the original nylon 66 material limits its further application in the field of engineering plastics, and the random distribution of carbon nanotubes in polymer matrix cannot fully exert its axial properties, and high content of carbon nanotubes leads to an increase in the viscosity of the resin. and high porosity.

Method used

The nylon 66 preparation method of unzipped carbon nanotubes carrying transition metal reinforced, by magnetically stirring and dispersing the transition metal salt and unzipped multi-wall carbon nanotubes in anhydrous ethanol, combined with ultrasonic treatment, the transition metal anchored unzipped carbon nanotubes are formed. The tube nanofiller was uniformly mixed by mechanical stirring and a twin screw extruder to prepare a modified nylon 66 material.

Benefits of technology

The mechanical properties of nylon 66 materials are improved, the surface energy of carbon nanotubes is reduced, its dispersion is enhanced, and the mechanical strength and Young's modulus of the material are significantly improved, which is 64% to 100% higher than the original nylon 66 strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116376275B_ABST
    Figure CN116376275B_ABST
Patent Text Reader

Abstract

The present invention discloses nylon 66 reinforced with transition metal carried by unzippered carbon nanotubes and a method thereof. The transition metal salt and unzippered multi-walled carbon nanotubes are dispersed in anhydrous ethanol respectively, dispersed by magnetic stirring, and mixed after being completely dispersed, and magnetic stirring and ultrasonication are performed to obtain transition metal anchored unzippered carbon nanotube nanofiller; transition metal anchored unzippered carbon nanotube nanofiller nylon 66 pellets are mixed uniformly by mechanical stirring, and the mixed material after being mixed uniformly is added to a twin-screw extruder at a uniform speed for melting heating and extrusion through a fine-diameter die to obtain unzippered carbon nanotube-carrying transition metal reinforced nylon 66 masterbatch. The preparation method of the unzippered multi-walled carbon nanotube anchored transition metal of the present invention is simple, and the unzippered multi-walled carbon nanotube anchored transition metal reinforced nylon 66 material reduces the surface energy of the carbon nanotubes by uniformly dispersing in a resin matrix, improves its dispersibility, and improves the mechanical properties of nylon 66 resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite materials, and in particular to an unzippered carbon nanotube-carried transition metal-reinforced nylon 66 and a method thereof. Background Art

[0002] Nylon 66 resin (PA66) is an excellent thermoplastic engineering material. Compared with other nylon series, nylon 66 has more hydrogen bonds, so it has excellent mechanical properties, high friction resistance, scratch resistance and solvent resistance, self-lubricating properties, shock absorption and sound absorption properties, and has become the most in-demand engineering plastic. It has been widely used in electronics, electrical and automotive industries, household appliances, sporting goods, etc. However, the low strength of the original nylon 66 greatly limits its further application. In order to make up for these defects, nylon 66 resin needs to be modified.

[0003] In recent years, many scholars at home and abroad have carried out a lot of research. Among them, carbon nanotubes, as a new type of nanomaterial, have the excellent characteristics of low density, large aspect ratio, high strength and high toughness. When added in a small amount, they can significantly improve the mechanical properties of the resin. Therefore, carbon nanotubes are considered to be an ideal reinforcement for composite materials and are expected to be used to strengthen the polymer matrix to improve its performance. If the content of carbon nanotubes is high, it will also cause the viscosity of the polymer resin to increase, making it difficult for the bubbles in it to escape, resulting in a high porosity of the hybrid material. In addition, carbon nanotubes are randomly distributed in the polymer matrix, and their axial properties cannot be fully exerted and utilized. Summary of the invention

[0004] In view of the defects in the prior art, the object of the present invention is to provide a nylon 66 reinforced with transition metals carried by unzippered carbon nanotubes and a method thereof.

[0005] To achieve the purpose, the technical solution provided by the present invention is:

[0006] A preparation method of unzippered carbon nanotubes carrying transition metal reinforced nylon 66 comprises the following steps: dispersing a transition metal salt and unzippered multi-walled carbon nanotubes in anhydrous ethanol respectively, dispersing them by magnetic stirring, mixing the two after they are completely dispersed, magnetically stirring and ultrasonicating them to obtain a transition metal anchored unzippered carbon nanotube nanofiller; mixing transition metal anchored unzippered carbon nanotube nanofiller nylon 66 pellets uniformly by mechanical stirring, adding the uniformly mixed mixture into a twin-screw extruder at a uniform speed for melt heating and extruding through a fine-diameter die to obtain a masterbatch of unzippered carbon nanotubes carrying transition metal reinforced nylon 66.

[0007] The preparation method comprises a transition metal salt comprising manganese chloride, indium acetate or cobalt nitrate, a mass ratio of the transition metal salt to the unzipped multi-walled carbon nanotube of 1:1, a magnetic stirring dispersion time of 2 hours, magnetic stirring for 2 hours and ultrasonication for 4 hours, and drying to obtain a transition metal anchored unzipped carbon nanotube nanofiller.

[0008] The preparation method uses Hummers technology to prepare multi-walled carbon nanotubes for unzipping, treats the original multi-walled carbon nanotubes with two strong acids HCl and HNO3 to remove impurities, and uses a strong oxidant KMnO4 to oxidize and tear the original carbon nanotubes to obtain unzipped multi-walled carbon nanotubes with a graphene sheet structure.

[0009] The preparation method uses Hummers technology to prepare the zipper, the diameter of the multi-walled carbon nanotubes MWCNTs used is 50nm, the length is 10μm, the ultrasonic stirring and dispersion time is 24h, the number of times potassium permanganate is added is 3 times, the amount of potassium permanganate used is 1.5g, the corresponding multi-walled carbon nanotube mass is 0.2g, and the insulation time after adding potassium permanganate is 4h.

[0010] In the preparation method, the mass content of the prepared modified nano filler doped into nylon 66 is 0.2%.

[0011] In the preparation method, the twin-screw extruder must ensure the dryness of the original nylon 66 masterbatch when feeding, and the feeding speed must be uniform to ensure uniform discharge. When using an injection molding machine for injection molding, the modified masterbatch must be dry and the feeding speed must be uniform.

[0012] The preparation method uses a twin-screw extruder to melt-extrude at a temperature of 260-280° C. and an extrusion speed of 20-60 rpm.

[0013] A nylon 66 hybrid material prepared according to any of the preparation methods.

[0014] After adopting the above technical solution, the present invention has the following beneficial effects: the preparation method of the unzipped multi-walled carbon nanotube anchored transition metal of the present invention is simple, and the unzipped multi-walled carbon nanotube anchored transition metal reinforced nylon 66 material is uniformly dispersed in the resin matrix, thereby reducing the surface energy of the carbon nanotube and improving its dispersibility. The presence of transition metal ions effectively transfers the stress applied to the nylon 66 resin matrix, thereby improving the mechanical properties of the nylon 66 resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The present invention is a flow chart of the preparation method of uMWCNTs-TM modified nylon 66 resin.

[0016] Figure 2TEM images of MWCNTs (a), uMWCNTs (b), and uMWCNTs-Mn (c).

[0017] Figure 3 SEM of the cross section of uMWCNTs-TM / nylon 66 hybrid material.

[0018] Figure 4 This is the tensile stress-strain curve of uMWCNTs-TM / PA66 composite material.

[0019] Figure 5 This is the Young's modulus curve of uMWCNTs-TM / PA66 composite material.

[0020] Figure 6 Diagram of the mechanism of enhanced mechanical properties in composite materials. DETAILED DESCRIPTION

[0021] The present invention is described in detail below in conjunction with specific embodiments.

[0022] Example 1

[0023] S1. Preparation of unzipped carbon nanotubes using a modified Hummers technique.

[0024] Specifically, 20 ml of nitric acid (HNO3) and 20 ml of concentrated sulfuric acid (98% H2SO4) were added to a 250 ml three-necked flask, 0.20 g of carbon nanotubes were weighed and added to the three-necked flask, the mixed solution was placed in a stirrer for mechanical stirring for 1 hour, then ultrasonically dispersed for 24 hours, and then 1.50 g of potassium permanganate (KMnO4) was added in 3 times, each time with an interval of 30 minutes. After that, the water bath was heated to 45°C and kept warm for 4 hours. 40 ml of pure water was measured, 1 ml of hydrogen peroxide (30% H2O2) was added, a hydrogen peroxide solution was prepared, and ice cubes were frozen. The ice cubes were placed in a beaker, and the mixed solution was added and stirred with a glass rod. This process was carried out in an ice water bath. Then, H2O2 (30%) was added dropwise to prevent the precipitation of insoluble MnO2 until no bubbles appeared, and a dezippered carbon nanotube dispersion was obtained. Perform multiple centrifugal washings. After the first centrifugation of the mixed solution, pour out the supernatant. During the second centrifugation, a certain proportion of HCl solution (the ratio of distilled water to concentrated sulfuric acid is 3:1) is required to wash the residual product of the test. The product obtained after the second centrifugation is centrifuged multiple times with pure water until the pH value of the supernatant is 7. After the centrifugal washing is completed, the washed unzipped multi-walled carbon nanotube dispersion is freeze-dried to collect the unzipped carbon nanotube powder.

[0025] S2. Preparation of uMWCNTs modified nylon 66 hybrid materials.

[0026] Take 0.04g uMWCNTs and disperse it in anhydrous ethanol solvent, add 20g nylon 66 masterbatch and mechanically stir it, put it into a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, and uniformly add the dried mixture to the twin-screw melt extrusion, the melt extrusion temperature is 260-280℃, the extrusion speed is 40rpm, cut it into slices after extrusion modification, put it into a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, and use an injection molding machine for injection molding, the injection melting temperature is 260-280℃, the injection pressure is 3MPa, and the mold temperature is 100℃. Figure 4 This is the tensile stress-strain curve of the composite material. The mechanical strength of uMWCNTs / PA66 material is enhanced by 64% compared with the original nylon 66. Figure 5 This is the Young's modulus curve of the composite material. The modulus of uMWCNTs-Mn / PA66 material is increased by 80% compared with the original nylon 66.

[0027] Example 2

[0028] S1. Preparation of uMWCNTs-Mn

[0029] Weigh 1g of manganese chloride (MnCl2·4H2O) solid and 1g of unzipped multi-walled carbon nanotube powder, place them in conical flasks respectively, add 10ml of anhydrous ethanol, stir magnetically for 2h, and after complete dispersion, mix the two solutions, stir the mixed solution magnetically for 2h, then ultrasonicate for 4h, and dry to obtain manganese-anchored unzipped carbon nanotube nanofiller powder uMWCNTs-Mn. Figure 2 (c) TEM image of uMWCNTs-Mn shows that the transition metal manganese has an irregular spherical structure and is successfully anchored to the side walls of uMWCNTs, indicating that the transition metal manganese ions are combined with uMWCNTs to form a new type of nanohybrid material.

[0030] S2. Preparation of uMWCNTs-Mn modified nylon 66 hybrid materials.

[0031] Take 0.04g uMWCNTs-Mn and disperse it in anhydrous ethanol solvent, add 20g nylon 66 masterbatch and stir mechanically, put it in a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, add the dried mixture to the twin screw for melt extrusion at a uniform speed, the melt extrusion temperature is 260-280℃, the extrusion speed is 40rpm, cut it into slices after extrusion modification, put it in a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, and use an injection molding machine for injection molding, the injection molding melt temperature is 260-280℃, the injection molding pressure is 3MPa, and the mold temperature is 100℃. The sample uMWCNTs-Mn (0.2%) / PA66 is obtained. Figure 4This is the tensile stress-strain curve of the composite material. The mechanical strength of uMWCNTs-Mn / PA66 material is enhanced by 74% compared with the original nylon 66. Figure 5 This is the Young's modulus curve of the composite material. The modulus of uMWCNTs-Mn / PA66 material is increased by 100% compared with the original nylon 66. Figure 6 Diagram of the mechanism of enhanced mechanical properties in composite materials.

[0032] Example 3

[0033] S1. Preparation of uMWCNTs-Co:

[0034] Weigh 1g of cobalt nitrate (Co(NO3)2·6H2O) solid and 1g of unzipped multi-walled carbon nanotube powder, place them in conical flasks respectively, add 10ml of anhydrous ethanol, stir magnetically for 2h, until they are completely dispersed, mix the two solutions, stir the mixed solution magnetically for 2h, then ultrasonicate for 4h, and dry to obtain cobalt-anchored unzipped carbon nanotube nanofiller powder uMWCNTs-Co.

[0035] S2. Preparation of uMWCNTs-Co modified nylon 66 hybrid materials.

[0036] Take 0.04g uMWCNTs-Co and disperse it in anhydrous ethanol solvent, add 20g nylon 66 masterbatch and stir mechanically, put it in a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, add the dried mixture to the twin screw for melt extrusion at a uniform speed, the melt extrusion temperature is 260-280℃, the extrusion speed is 40rpm, cut it into slices after extrusion modification, put it in a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, and use an injection molding machine for injection molding, the injection molding melt temperature is 260-280℃, the injection molding pressure is 3MPa, and the mold temperature is 100℃. The sample uMWCNTs-Co (0.2%) / PA66 is obtained. Figure 4 This is the tensile stress-strain curve of the composite material. The mechanical strength of uMWCNTs-Co / PA66 material is enhanced by 55% compared with the original nylon 66. Figure 5 This is the Young's modulus curve of the composite material. The modulus of uMWCNTs-Co / PA66 material is increased by 70% compared with the original nylon 66.

[0037] Example 4

[0038] S1. Preparation of uMWCNTs-Ln:

[0039] Weigh 1g of indium acetate (In(C2H3O2)3) solid and 1g of unzipped multi-walled carbon nanotube powder, place them in conical flasks respectively, add 10ml of anhydrous ethanol, stir magnetically for 2h, until they are completely dispersed, mix the two solutions, stir the mixed solution magnetically for 2h, then ultrasonicate for 4h, and dry to obtain indium-anchored unzipped carbon nanotube nanofiller powder uMWCNTs-Ln.

[0040] S2. Preparation of uMWCNTs-Ln modified nylon 66 hybrid materials.

[0041] Take 0.04g uMWCNTs-Ln and disperse it in anhydrous ethanol solvent, add 20g nylon 66 masterbatch and stir mechanically, put it in a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, add the dried mixture to the twin screw for melt extrusion at a uniform speed, the melt extrusion temperature is 260-280℃, the extrusion speed is 40rpm, cut it into slices after extrusion modification, put it in a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, and use an injection molding machine for injection molding, the injection molding melt temperature is 260-280℃, the injection molding pressure is 3MPa, and the mold temperature is 100℃. The sample uMWCNTs-Ln (0.2%) / PA66 is obtained. Figure 4 This is the tensile stress-strain curve of the composite material. The mechanical strength of uMWCNTs-Ln / PA66 material is enhanced by 45% compared with the original nylon 66. Figure 5 This is the Young's modulus curve of the composite material. The modulus of uMWCNTs-Ln / PA66 material is increased by 53% compared with the original nylon 66.

[0042] Comparative Example 1:

[0043] S1. Preparation of original nylon 66 material.

[0044] Take 20g of nylon 66 masterbatch, stir it mechanically, put it into a vacuum drying oven, dry it at 80℃ for 12h, dry it at 120℃ for 4h, and use an injection molding machine to mold it, with the injection melting temperature of 260-280℃, the injection pressure of 3MPa, and the mold temperature of 100℃ to obtain the sample PA66.

[0045] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.

Claims

1. A method for preparing unzippered carbon nanotubes carrying transition metals reinforced nylon 66, characterized in that: The transition metal salt and the unzippered multi-walled carbon nanotubes are dispersed in anhydrous ethanol respectively, dispersed by magnetic stirring, and mixed after complete dispersion, and magnetically stirred and ultrasonicated to obtain a transition metal anchored unzippered carbon nanotube nanofiller; the transition metal anchored unzippered carbon nanotube nanofiller nylon 66 pellets are mixed evenly by mechanical stirring, and the mixed material after mixing evenly is uniformly added to a twin-screw extruder for melt heating and extruded through a fine-diameter die to obtain an unzippered carbon nanotube-carrying transition metal reinforced nylon 66 masterbatch; the transition metal salt is manganese chloride, manganese chloride The mass ratio of manganese to unzipped multi-walled carbon nanotubes is 1:1, the magnetic stirring dispersion time is 2 hours, after magnetic stirring for 2 hours and ultrasonication for 4 hours, the unzipped carbon nanotube nanofiller anchored by transition metal is obtained after drying; the preparation method of the unzipped multi-walled carbon nanotubes is as follows: unzipped multi-walled carbon nanotubes are prepared by using a modified Hummers technique, the original multi-walled carbon nanotubes are treated with two strong acids HCl and HNO3 to remove impurities, and the original carbon nanotubes are oxidized and torn with a strong oxidant KMnO4 to obtain unzipped multi-walled carbon nanotubes with a graphene sheet structure.

2. The preparation method according to claim 1, characterized in that: When the modified Hummers technique is used to prepare unzipped multi-walled carbon nanotubes, the diameter of the multi-walled carbon nanotubes MWCNTs used is 50nm, the length is 10μm, the ultrasonic stirring and dispersion time is 24h, the number of times potassium permanganate is added is 3 times, the amount of potassium permanganate used is 1.5g, the corresponding mass of the multi-walled carbon nanotubes is 0.2g, and the insulation time after adding potassium permanganate is 4h.

3. The preparation method according to claim 1, characterized in that: The prepared modified nanofiller was doped into nylon 66 with a mass content of 0.2%.

4. The preparation method according to claim 1, characterized in that: When feeding the twin-screw extruder, it is necessary to ensure the dryness of the original nylon 66 masterbatch, and also ensure that the feeding speed is uniform to ensure uniform discharge.

5. The preparation method according to claim 1, characterized in that: The temperature of melt extrusion using a twin-screw extruder is 260-280°C and the extrusion speed is 20-60rpm.

6. Nylon 66 hybrid material prepared according to any one of the preparation methods of claims 1-5.