A solid perovskite quantum dot composite material and its preparation method and application
By using silane coupling agent containing halogen atoms to form a halogen-rich environment during the synthesis of solid perovskite quantum dots, the problem of poor thermal stability of solid perovskite quantum dots is solved, and its water and thermal stability is improved.
Patent Information
- Application Number
- CN202310367610.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-04-07
AI Technical Summary
The prior art is difficult to maintain a halogen-rich environment in solid perovskite quantum dots, resulting in poor thermal stability and ineffective improvement of water and thermal stability in practical applications.
During the synthesis of solid perovskite quantum dots, silane coupling agent containing halogen atoms is added as the halogen source. Through hydrolysis and crosslinking of silane coupling agent, a multi-dentate ligand passivation of the halogen surface of perovskite quantum dots is formed. Vacancy defects and form a halogen-rich environment around solid perovskite quantum dots, improving its water and thermal stability.
It significantly improves the water stability and thermal stability of solid perovskite quantum dots, so that they can show higher light emission efficiency and better long-term stability in practical applications.
Smart Images

Figure CN116376547B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of quantum dot materials, and in particular relates to a solid perovskite quantum dot composite material and a preparation method and application thereof. Background Art
[0002] In recent years, perovskite quantum dots have attracted attention and research due to their excellent optical properties. Compared with traditional inorganic semiconductor colloidal quantum dots, perovskite quantum dots have the advantages of wider fluorescence emission range, simple synthesis, and low price. They have great application prospects in lighting, display, lasers, solar cells and other fields.
[0003] Due to the ionic compound properties of perovskite quantum dots, in addition to the influence of polar environments, the changes in lattice distortion and the shedding of surface ligands also have a great impact on their luminescence properties. The surface ligands of perovskite quantum dots can prevent quantum dots from aggregating in a high temperature environment, regulate nucleation growth, and control the size and shape of quantum dots. The protonated oleylamine ligands on the surface of perovskite quantum dots undergo a dynamic combination of shedding and adsorption. When they shed off, it is very easy to cause the shedding of surface halogens and form halogen vacancies on the surface of perovskite quantum dots, which in turn leads to a rapid decrease in quantum yield and poor stability. In addition, the use of polar antisolvents during the purification process may also cause the Br ions on the surface of perovskite quantum dots to be stripped, resulting in the generation of halogen vacancies.
[0004] To this end, studies have shown that directly adding an appropriate amount of metal halogen compound salts to the quantum dot solution can significantly improve the stability of perovskite quantum dots and maintain a high PLQY. Woo et al. (DOI: 10.1021 / acs.chemmater.7b02669) not only used PbBr2 as a precursor during the synthesis process, but also added ZnBr2 to provide a halogen-rich environment, thereby effectively enhancing the stability of perovskite quantum dots; subsequently, Narayan Pradhan et al. (DOI: 10.1021 / acs.jpclett.8b03047) passivated the surface defects of perovskite quantum dots by post-treatment with 9 types of halide salts, greatly improving the stability and PLQY of perovskite quantum dots. However, in the actual application of perovskite quantum dots, the halogen-rich environment of the solution method cannot be maintained in solid-state applications.
[0005] The existing way to improve the environmental stability of solid-state perovskite quantum dots is to coat the surface of the perovskite quantum dots with a layer of SiO2 or some hydrophobic polymers. Guo et al. (DOI: 10.1016 / j.matlet.2020.128041) proposed to coat the surface of the perovskite quantum dots with a layer of TiO2 shell; Tang et al. (DOI: 10.1002 / smll.201900484) proposed that the surface of the perovskite quantum dots was coated with a layer of SiO2 by TEOS hydrolysis; Wang et al. (DOI: 10.1007 / s12274-023-5489-1) obtained a better water stability effect through multiple coatings such as TMOS, APTES and Ps. However, the existing coating technology can only unilaterally improve the water stability of solid-state perovskite quantum dots, but has no effect on improving thermal stability. Studies have shown that in actual applications, the reason why perovskite quantum dots have poor thermal stability during the aging process is that the presence of thermally activated halogen vacancies in solid-state perovskite quantum dots makes it impossible to ensure a halogen-rich environment.
[0006] Therefore, how to maintain a halogen-rich environment for solid-state perovskite quantum dots in practical applications to improve the thermal stability of solid-state perovskite quantum dots is a technical problem that needs to be solved urgently. Summary of the invention
[0007] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a solid perovskite quantum dot composite material and a preparation method and application thereof. The present invention adds a silane coupling agent containing halogen atoms as a halogen source during the synthesis process of the solid perovskite quantum dot composite material, which can not only provide a sufficient halogen source to form a stable multi-dentate ligand to passivate the halogen vacancy sites of the perovskite quantum dots, but also form a halogen-rich environment around the solid perovskite quantum dots, thereby improving the water stability of the solid perovskite quantum dots and further improving the thermal stability.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a solid perovskite quantum dot composite material, the preparation method comprising the following steps:
[0010] (1) mixing a lead source, a cesium source and a ligand in a solvent to react to obtain a perovskite quantum dot precursor reaction solution;
[0011] (2) Mixing the perovskite quantum dot precursor solution and a silane coupling agent containing halogen atoms, reacting, cooling, and hydrolyzing to obtain the solid perovskite quantum dot composite material.
[0012] The present invention adds a silane coupling agent containing halogen atoms as a halogen source during the synthesis process of a solid perovskite quantum dot composite material. During the reaction process, the -CX bond (X is a halogen atom) in the silane coupling agent is broken, which can provide a halogen source for the solid perovskite quantum dots and participate in the synthesis of the perovskite quantum dots. After the quantum dots are nucleated and crystallized, the silane coupling agent can be used as a passivating agent to passivate the halogen vacancy defects on the surface of the solid perovskite quantum dots in the form of -CX-Pb coordination bonds, and the monodispersed silane coupling agent is hydrolyzed and cross-linked, which makes it possible for multiple silane coupling agents containing halogen atoms to passivate the surface of the perovskite quantum dots to form multi-dentate ligand passivation. In addition, the abundant silane coupling agent can form a halogen-rich environment around the solid perovskite quantum dots, thereby obtaining a solid perovskite quantum dot composite material with significantly improved water stability and thermal stability.
[0013] And / or, the lead source in step (1) includes any one of lead oxide, lead acetate or lead carbonate.
[0014] And / or, the cesium source in step (1) includes any one of cesium carbonate or cesium acetate.
[0015] And / or, the molar ratio of the lead source to the cesium source in step (1) is 1:(0.25-2), for example, it can be 1:0.25, 1:0.5, 1:0.75, 1:1, 1:1.25, 1:1.5, 1:1.75 or 1:2, etc.
[0016] And / or, the ligand in step (1) comprises an organic acid and an organic amine;
[0017] And / or, the organic acid includes any one or a combination of at least two of dodecylbenzenesulfonic acid, oleic acid or octanoic acid;
[0018] And / or, the organic amine includes oleylamine and / or n-octylamine;
[0019] And / or, the ligand in step (1) comprises oleic acid and oleylamine, and the molar ratio of oleic acid to oleylamine is (0.25-4):1, for example, it can be 0.25:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1 or 4:1, etc., preferably (1-1.5):1.
[0020] In the present invention, if the molar ratio of oleic acid to oleylamine is too large, that is, the content of oleic acid is too much, the catalytic environment for the hydrolysis, condensation and cross-linking of the silane coupling agent containing halogen atoms will be an acidic environment, which can assist the dissolution of the quantum dot precursor material and alleviate the flocculation of the quantum dots, thereby obtaining a gel-like perovskite quantum dot composite material; if the molar ratio of oleic acid to oleylamine is too small, that is, the content of oleic acid is too small, the catalytic environment for the hydrolysis, condensation and cross-linking of the silane coupling agent containing halogen atoms will be an alkaline environment, which will cause the size of the final nucleated quantum dots to be too small, the emission to be blue-shifted, and a powdery perovskite quantum dot composite material to be obtained.
[0021] And / or, the solvent in step (1) includes any one of 1-octadecene, liquid paraffin or trioctylphosphine oxide, or a combination of at least two thereof.
[0022] And / or, the reaction in step (1) is accompanied by stirring.
[0023] And / or, the reaction environment in step (1) is a vacuum environment.
[0024] And / or, the reaction temperature in step (1) is 80-110°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 110°C or 120°C.
[0025] And / or, the reaction time of step (1) is 20-40 min, for example, it can be 20 min, 22 min, 24 min, 26 min, 28 min, 30 min, 32 min, 34 min, 36 min, 38 min or 40 min, etc.
[0026] And / or, the silane coupling agent containing halogen atoms in step (2) includes 3-Xpropyltrimethoxysilane and / or 3-X'propyltriethoxysilane, wherein X and X' independently include any one of bromine atoms, iodine atoms or chlorine atoms or a combination of at least two thereof.
[0027] And / or, the molar ratio of the halogen-containing silane coupling agent in step (2) to the lead source in step (1) is (3-20):1, for example, 3:1, 6:1, 9:1, 12:1, 15:1, 18:1 or 20:1, etc., preferably (4-16):1.
[0028] In the present invention, if the molar ratio of the silane coupling agent containing halogen atoms to the lead source is too small, that is, the amount of the silane coupling agent containing halogen atoms is too little, the prepared perovskite quantum dot composite material has a low PLQY and poor thermal stability; if the molar ratio of the silane coupling agent containing halogen atoms to the lead source is too large, that is, the amount of the silane coupling agent containing halogen atoms is too much, the initial PLQY of the prepared quantum dot composite material is not high. This is because when there is too much silane coupling agent, a thick SiO2 shell layer will be formed around the quantum dots, which affects the absorption of the quantum dots and further weakens the emission of the quantum dots.
[0029] And / or, the mixing method in step (2) includes:
[0030] A silane coupling agent containing halogen atoms and an organic solvent are mixed to obtain a diluent, and the diluent is mixed with the perovskite quantum dot precursor solution.
[0031] The purpose of pre-diluting the silane coupling agent containing halogen atoms in the present invention is to reduce the concentration of the silane coupling agent containing halogen atoms, thereby reducing the reaction rate and making the nucleation of the synthesized perovskite quantum dots more uniform.
[0032] And / or, the organic solvent includes any one of 1-octadecene, liquid paraffin or trioctylphosphine oxide, or a combination of at least two thereof.
[0033] And / or, the mixing in step (2) is carried out in a protective atmosphere.
[0034] The present invention does not limit the selection of the gas in the protective atmosphere, and illustratively, it may be nitrogen.
[0035] And / or, the reaction temperature in step (2) is 160-230°C, for example, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C or 230°C.
[0036] In the present invention, if the reaction temperature is too low, the PLQY of the obtained perovskite quantum dots is low; if the reaction temperature is too high, there is a safety risk.
[0037] And / or, the reaction time of step (2) is 2-4 min, for example, it can be 2 min, 2.2 min, 2.4 min, 2.6 min, 2.8 min, 3 min, 3.2 min, 3.4 min, 3.6 min, 3.8 min or 4 min, etc.
[0038] And / or, step (2) cooling to room temperature.
[0039] It should be noted that the room temperature is 25±5°C, for example, it can be 20°C, 22°C, 24°C, 26°C, 28°C or 30°C.
[0040] In the present invention, after cooling to room temperature, the silane coupling agent containing halogen atoms will undergo hydrolysis, condensation and cross-linking, which will not only make it possible for multiple silane coupling agents to passivate the surface of the perovskite quantum dots to form multidentate ligand passivation, but also after the hydrolysis and cross-linking are completed, a stable silicon dioxide coating layer will be formed on the surface of the perovskite quantum dots, thus obtaining a solid perovskite quantum dot composite material.
[0041] And / or, the hydrolysis in step (2) is carried out in a natural environment.
[0042] In the present invention, the hydrolysis is carried out in a natural environment, that is, the reaction container is left open.
[0043] And / or, the hydrolysis process in step (2) is accompanied by stirring.
[0044] And / or, the hydrolysis time in step (2) is 2-10 h, for example, it can be 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.
[0045] In the present invention, if the hydrolysis time is too short, the hydrolysis and cross-linking of the silane coupling agent of the halogen atom will be incomplete, and the water stability of the perovskite quantum dot composite material will be poor; if the hydrolysis time is too long, a dense perovskite quantum dot composite material can be formed, but if the time is too long, the entire synthesis process will be relatively long, increasing the time cost.
[0046] As a preferred technical solution, the preparation method comprises the following steps:
[0047] (I) mixing a lead source, a cesium source and a ligand in a solvent in a vacuum environment at 80-110° C. and stirring for 20-40 minutes to obtain a perovskite quantum dot precursor solution;
[0048] Wherein, the molar ratio of the lead source to the cesium source is 1:(0.25-2), the ligand includes oleic acid and oleylamine, and the molar ratio of oleic acid to oleylamine is (0.25-4):1;
[0049] (II) mixing a silane coupling agent containing a halogen atom and an organic solvent to obtain a diluted solution;
[0050] Wherein, the organic solvent includes any one or a combination of at least two of 1-octadecene, liquid paraffin or trioctylphosphine oxide;
[0051] (III) injecting the diluted solution into the perovskite quantum dot precursor solution under a protective atmosphere at 160-230° C. and reacting for 2-4 minutes, cooling to room temperature, stirring in an open air for 2-10 hours for hydrolysis, and obtaining the solid perovskite quantum dot composite material after centrifugation;
[0052] Wherein, the molar ratio of the silane coupling agent containing halogen atoms to the lead source is (3-20):1.
[0053] In a second aspect, the present invention provides a solid-state perovskite quantum dot composite material, wherein the solid-state perovskite quantum dot composite material is prepared by the preparation method described in the first aspect;
[0054] The solid-state perovskite quantum dot composite material comprises perovskite quantum dots and SiO2 coated on the surface of the perovskite quantum dots.
[0055] In the present invention, the SiO2 coated on the surface of the perovskite quantum dots may be a SiO2 gel or a SiO2 ball matrix.
[0056] In a third aspect, the present invention provides an application of the solid-state perovskite quantum dot composite material as described in the second aspect, wherein the solid-state perovskite quantum dot composite material is applied in the fields of lighting, display, laser and solar cell.
[0057] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0058] Compared with the prior art, the present invention has the following beneficial effects:
[0059] The present invention adds a silane coupling agent containing halogen atoms as a halogen source during the synthesis process of the solid-state perovskite quantum dot composite material, which can not only provide a sufficient halogen source to form a stable multi-dentate ligand to passivate the halogen vacancy sites of the perovskite quantum dots, but also form a halogen-rich environment around the solid-state perovskite quantum dots, thereby improving the water stability of the solid-state perovskite quantum dots and further improving the thermal stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is a diagram showing the reaction mechanism of the silane coupling agent containing halogen atoms in Example 1 of the present invention. DETAILED DESCRIPTION
[0061] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0062] It should be noted that in the following examples, room temperature refers to 25°C.
[0063] Example 1
[0064] This embodiment provides a method for preparing a solid perovskite quantum dot composite material, the preparation method comprising the following steps:
[0065] (1) In a vacuum environment at 100° C., 0.0446 g of a lead source, 0.0324 g of a cesium source, and a ligand were mixed in 10 mL of a solvent and stirred for 30 min to obtain a perovskite quantum dot precursor solution;
[0066] Wherein, the lead source is lead oxide, the cesium source is cesium carbonate, the molar ratio of lead oxide to cesium carbonate is 1:0.5, the ligand comprises oleic acid and oleylamine in a molar ratio of 1.2:1, and the solvent is 1-octadecene;
[0067] (2) mixing 400 μL of a silane coupling agent containing a halogen atom and 500 μL of an organic solvent to obtain a diluent;
[0068] Wherein, the silane coupling agent containing halogen atoms is 3-bromopropyltriethoxysilane, and the organic solvent is 1-octadecene;
[0069] (3) In a nitrogen atmosphere at 200° C., injecting the diluted solution into the perovskite quantum dot precursor solution using a needle syringe and reacting for 3 minutes, cooling to room temperature, stirring in an open air for 8 hours for hydrolysis, and naturally standing for 24 hours after the stirring to obtain a gel-state perovskite quantum dot composite material, that is, a solid-state perovskite quantum dot composite material, wherein the solid-state perovskite quantum dot composite material includes perovskite quantum dots and SiO2 gel coated on the surface of the perovskite quantum dots;
[0070] The molar ratio of the silane coupling agent containing halogen atoms to the lead source is 8:1.
[0071] Figure 1 The diagram shows the reaction mechanism of the silane coupling agent containing halogen atoms in this embodiment. It can be seen from the figure that the silane coupling agent containing halogen atoms will passivate the halogen vacancy defects on the surface of the perovskite quantum dots in the form of -CX-Pb coordination bonds (X represents the halogen atom) as a passivator, and then further hydrolyze and cross-link, which makes it possible for multiple silane coupling agents containing halogen atoms to passivate the surface of the perovskite quantum dots to form multi-dentate ligand passivation; in addition, abundant silane coupling agents can form a halogen-rich environment around the solid perovskite quantum dots, thereby obtaining a solid perovskite quantum dot composite material with significantly improved water stability and thermal stability.
[0072] Example 2
[0073] The difference between this embodiment and embodiment 1 is that the silane coupling agent containing halogen atoms in step (2) is 3-bromopropyltrimethoxysilane.
[0074] The rest of the preparation methods and parameters were the same as those in Example 1.
[0075] Example 3
[0076] The difference between this embodiment and embodiment 1 is that the silane coupling agent containing halogen atoms in step (2) is 3-chloropropyltriethoxysilane.
[0077] The rest of the preparation methods and parameters were the same as those in Example 1.
[0078] Example 4
[0079] The difference between this embodiment and embodiment 1 is that the silane coupling agent containing halogen atoms in step (2) is 3-chloropropyltrimethoxysilane.
[0080] The rest of the preparation methods and parameters were the same as those in Example 1.
[0081] Example 5
[0082] The difference between this embodiment and embodiment 1 is that the silane coupling agent containing halogen atoms in step (2) is 3-iodopropyltriethoxysilane.
[0083] The rest of the preparation methods and parameters were the same as those in Example 1.
[0084] Example 6
[0085] The difference between this embodiment and embodiment 1 is that the silane coupling agent containing halogen atoms in step (2) is 3-iodopropyltrimethoxysilane.
[0086] The rest of the preparation methods and parameters were the same as those in Example 1.
[0087] Example 7
[0088] This embodiment provides a method for preparing a solid perovskite quantum dot composite material, the preparation method comprising the following steps:
[0089] (1) In a vacuum environment at 80° C., 0.0267 g of a lead source, 0.0326 g of a cesium source, and a ligand were mixed in 10 mL of a solvent and stirred for 40 min to obtain a perovskite quantum dot precursor solution;
[0090] Wherein, the lead source is lead carbonate, the cesium source is cesium carbonate, the molar ratio of lead carbonate to cesium carbonate is 1:1, the ligand comprises oleic acid and oleylamine in a molar ratio of 0.6:1, and the solvent is liquid paraffin;
[0091] (2) mixing 150 μL of a silane coupling agent containing a halogen atom and 500 μL of an organic solvent to obtain a diluent;
[0092] Wherein, the silane coupling agent containing halogen atoms is 3-bromopropyltriethoxysilane, and the organic solvent is liquid paraffin;
[0093] (3) In a nitrogen atmosphere at 160° C., injecting the diluted solution into the perovskite quantum dot precursor solution using a needle syringe and reacting for 4 minutes, cooling to room temperature, stirring in an open air for 2 hours for hydrolysis, centrifuging after the stirring, washing the precipitate obtained by centrifugation with n-hexane three times, and vacuum drying at 65° C. for 8 hours to obtain a powdered perovskite quantum dot composite material, i.e., a solid perovskite quantum dot composite material, wherein the solid perovskite quantum dot composite material includes perovskite quantum dots and a SiO2 ball matrix coated on the surface of the perovskite quantum dots;
[0094] The molar ratio of the silane coupling agent containing halogen atoms to the lead source is 3:1.
[0095] Example 8
[0096] This embodiment provides a method for preparing a solid perovskite quantum dot composite material, the preparation method comprising the following steps:
[0097] (1) In a vacuum environment at 110° C., 0.0325 g of a lead source, 0.0384 g of a cesium source, and a ligand were mixed in 10 mL of a solvent and stirred for 20 min to obtain a perovskite quantum dot precursor solution;
[0098] Wherein, the lead source is lead acetate, the cesium source is cesium acetate, the molar ratio of lead acetate to cesium acetate is 1:2, the ligand comprises oleic acid and oleylamine in a molar ratio of 4:1, and the solvent is trioctyl phosphine oxide;
[0099] (2) mixing 1000 μL of a silane coupling agent containing a halogen atom and 1 mL of an organic solvent to obtain a diluent;
[0100] Wherein, the silane coupling agent containing halogen atoms is 3-bromopropyltriethoxysilane, and the organic solvent is trioctylphosphine oxide;
[0101] (3) In a nitrogen atmosphere at 230° C., injecting the diluted solution into the perovskite quantum dot precursor solution using a needle syringe and reacting for 2 minutes, cooling to room temperature, stirring in an open air for 10 hours for hydrolysis, and naturally standing for 24 hours after the stirring to obtain a gel-state perovskite quantum dot composite material, that is, a solid-state perovskite quantum dot composite material, wherein the solid-state perovskite quantum dot composite material includes perovskite quantum dots and SiO2 gel coated on the surface of the perovskite quantum dots;
[0102] The volume ratio of the silane coupling agent containing halogen atoms to the mixed solution is 20:1.
[0103] Example 9
[0104] The difference between this embodiment and embodiment 1 is that the molar ratio of the silane coupling agent containing halogen atoms to the lead source is 25:1.
[0105] The rest of the preparation methods and parameters were the same as those in Example 1.
[0106] Example 10
[0107] The difference between this embodiment and embodiment 1 is that the molar ratio of the silane coupling agent containing halogen atoms to the lead source is 2:1.
[0108] The rest of the preparation methods and parameters were the same as those in Example 1.
[0109] Embodiment 11
[0110] The difference between this embodiment and embodiment 1 is that the dilution solution in step (3) is injected into the perovskite quantum dot precursor solution and the reaction temperature is 120°C.
[0111] The rest of the preparation methods and parameters were the same as those in Example 1.
[0112] Example 12
[0113] The difference between this embodiment and embodiment 1 is that the dilution solution in step (3) is injected into the perovskite quantum dot precursor solution and the reaction temperature is 250°C.
[0114] The rest of the preparation methods and parameters were the same as those in Example 1.
[0115] Example 13
[0116] The difference between this embodiment and embodiment 1 is that the hydrolysis time in step (3) is 2 hours.
[0117] The rest of the preparation methods and parameters were the same as those in Example 1.
[0118] Embodiment 14
[0119] The difference between this embodiment and embodiment 1 is that the hydrolysis time in step (3) is 12 hours.
[0120] The rest of the preparation methods and parameters were the same as those in Example 1.
[0121] Comparative Example 1
[0122] The difference between this comparative example and Example 1 is that the silane coupling agent containing halogen atoms in step (2) is replaced by trimethylsilyl bromide.
[0123] The rest of the preparation methods and parameters were the same as those in Example 1.
[0124] Comparative Example 2
[0125] The difference between this comparative example and Example 1 is that the hydrolysis step in step (3) is omitted.
[0126] The rest of the preparation methods and parameters were the same as those in Example 1.
[0127] Comparative Example 3
[0128] The difference between this comparative example and Example 1 is that the hydrolysis is carried out in a closed environment, that is, after the reaction is completed and the temperature is lowered to room temperature, the hydrolysis is carried out in a closed environment.
[0129] The rest of the preparation methods and parameters were the same as those in Example 1.
[0130] Performance Testing
[0131] The solid-state perovskite quantum dot composite materials prepared in Examples 1-14 and Comparative Examples 1-3 were tested for water stability and thermal stability.
[0132] The perovskite quantum dot composite material is mixed with polydimethylsiloxane (PDMS) material, and then dried in an oven at 85°C for 30 minutes to prepare a PDMS film, wherein the mass ratio of the perovskite quantum dot composite material to the PDMS material is 1:32;
[0133] The conditions for the water stability test are as follows: the PDMS membrane is placed in an aqueous solution and stored at room temperature and away from light;
[0134] The thermal stability test conditions are as follows: the PDMS film is placed in a constant temperature oven at 85°C.
[0135] The results of the thermal stability test are shown in Table 1, and the results of the water stability test are shown in Table 2.
[0136] Table 1
[0137]
[0138]
[0139] Table 2
[0140]
[0141]
[0142] analyze:
[0143] As can be seen from the above table, the present invention adds a silane coupling agent containing halogen atoms as a halogen source during the synthesis of the solid-state perovskite quantum dot composite material, which can not only provide a sufficient halogen source to form a stable multi-dentate ligand to passivate the halogen vacancy sites of the perovskite quantum dots, but also form a halogen-rich environment around the solid-state perovskite quantum dots, thereby improving the water stability of the solid-state perovskite quantum dots and further improving the thermal stability.
[0144] By comparing the data results of Example 1 with those of Examples 9-10, it can be seen that if the molar ratio of the silane coupling agent containing halogen atoms to the lead source is too small, the perovskite quantum dot composite material will not have a halogen-rich environment or even lack halogen, which will lead to poor thermal stability; if the molar ratio of the silane coupling agent containing halogen atoms to the lead source is too large, a thick SiO2 shell will be formed around the perovskite quantum dots, affecting the absorption of the perovskite quantum dot composite material, thereby resulting in a lower PLQY of the perovskite quantum dot composite material.
[0145] By comparing the data results of Example 1 with those of Examples 11-12, it can be seen that when the temperature is too low, the diluted solution is injected into the perovskite quantum dot precursor solution and reacts, the nucleation temperature of the quantum dots is low and the quantum dots have not yet completed nucleation and crystallization, thereby causing the PLQY to decrease; when the temperature is too high, the diluted solution is injected into the perovskite quantum dot precursor solution and reacts, except for the quenching of the quantum dots in the high temperature environment, there is no significant abnormality in the PLQY after room temperature, and the stability difference is not large, but there is a certain safety risk.
[0146] By comparing the data results of Example 1 with those of Examples 13-14, it can be seen that if the hydrolysis time is too short, the outer layer coating of the quantum dots will not be good, which will lead to poor water stability and thermal stability, especially extremely poor water stability; and if the hydrolysis time is too long, in addition to the relatively long synthesis process, there is not much difference in the hydrothermal stability performance of the quantum dots.
[0147] From the comparison of the data results of Example 1 and Comparative Example 1, it can be seen that if trimethylsilyl bromide in the prior art is used, since trimethylsilyl bromide is only used as a precursor for synthesizing quantum dots as a bromine source, the outer layer cannot form a composite shell structure, which leads to extremely poor stability.
[0148] From the comparison of the data results of Example 1 and Comparative Example 2, it can be seen that if the hydrolysis step is not performed, there is no shell structure generated by hydrolysis around the quantum dots, and the stability effect is not good.
[0149] From the comparison of the data results of Example 1 and Comparative Example 3, it can be seen that if the hydrolysis is carried out in a closed environment, the hydrolysis process is quite slow, resulting in the shell structure formed around the quantum dots not being dense and the final stability being poor.
[0150] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a solid perovskite quantum dot composite material, characterized in that: The preparation method comprises the following steps: (1) mixing a lead source, a cesium source and a ligand in a solvent to react to obtain a perovskite quantum dot precursor solution; (2) mixing a silane coupling agent containing a halogen atom and an organic solvent to obtain a diluted solution; (3) injecting the diluted solution into the perovskite quantum dot precursor solution at 160-230° C., reacting, cooling, and performing open hydrolysis to obtain the solid perovskite quantum dot composite material; The molar ratio of the silane coupling agent containing halogen atoms in step (2) to the lead source in step (1) is (3-20):
1.
2. The preparation method according to claim 1, characterized in that: The lead source in step (1) includes any one of lead oxide, lead acetate or lead carbonate; And / or, the cesium source in step (1) includes any one of cesium carbonate or cesium acetate; And / or, the molar ratio of the lead source to the cesium source in step (1) is 1:(0.25-2); And / or, the ligand in step (1) comprises an organic acid and an organic amine; And / or, the organic acid includes any one or a combination of at least two of dodecylbenzenesulfonic acid, oleic acid or n-octanoic acid; And / or, the organic amine includes oleylamine and / or octylamine; And / or, the ligand in step (1) comprises oleic acid and oleylamine, and the molar ratio of oleic acid to oleylamine is (0.25-4):1; And / or, the solvent in step (1) comprises any one of 1-octadecene, liquid paraffin or trioctylphosphine oxide, or a combination of at least two thereof.
3. The preparation method according to claim 2, characterized in that: The ligand in step (1) comprises oleic acid and oleylamine, and the molar ratio of oleic acid to oleylamine is (1-1.5):
1.
4. The preparation method according to claim 1, characterized in that: The reaction in step (1) is accompanied by stirring; And / or, the reaction environment in step (1) is a vacuum environment; And / or, the reaction temperature in step (1) is 80-110°C.
5. The preparation method according to claim 1, characterized in that: The silane coupling agent containing halogen atoms in step (2) includes 3-X propyltrimethoxysilane and / or 3-X' propyltriethoxysilane, wherein X and X' independently include any one of bromine, iodine or chlorine; And / or, the molar ratio of the silane coupling agent containing halogen atoms in step (2) to the lead source in step (1) is (4-16):
1.
6. The preparation method according to claim 1, characterized in that: In a protective atmosphere, the diluted solution is injected into a perovskite quantum dot precursor solution to carry out a reaction.
7. The preparation method according to claim 1, characterized in that: Step (3) is cooling to room temperature.
8. The preparation method according to claim 1, characterized in that: The hydrolysis time in step (3) is 2-10 hours.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: (I) In a vacuum environment at 80-110° C., a lead source, a cesium source and a ligand are mixed in a solvent and stirred for 20-40 minutes to react to obtain a perovskite quantum dot precursor solution; Wherein, the molar ratio of the lead source to the cesium source is 1:(0.25-2), the ligand includes oleic acid and oleylamine, and the molar ratio of oleic acid to oleylamine is (0.25-4):1; (II) mixing a silane coupling agent containing a halogen atom and an organic solvent to obtain a diluent; Wherein, the organic solvent includes any one or a combination of at least two of 1-octadecene, liquid paraffin or trioctylphosphine oxide; (III) In a protective atmosphere at 160-230° C., injecting the diluted solution into the perovskite quantum dot precursor solution and reacting for 2-4 minutes, cooling to room temperature, stirring in an open air for 2-10 hours for hydrolysis, and obtaining the solid perovskite quantum dot composite material after centrifugation; Wherein, the molar ratio of the silane coupling agent containing halogen atoms to the lead source is (3-20):
1.
10. A solid perovskite quantum dot composite material, characterized in that: The solid-state perovskite quantum dot composite material is prepared by the preparation method according to any one of claims 1 to 9; The solid-state perovskite quantum dot composite material comprises perovskite quantum dots and SiO2 coated on the surface of the perovskite quantum dots; The SiO2 is a SiO2 gel or SiO2 ball matrix.
11. A use of the solid perovskite quantum dot composite material as claimed in claim 10, characterized in that: The solid-state perovskite quantum dot composite material is used in the fields of lighting, display, laser and solar cell.