A kind of as-cast ultra-low temperature ductile iron and production method thereof
By using materials such as silicon magnesium alloy and rare earth spheroidizer in ductile iron, combined with specific process steps, the problem of deterioration of ductile iron in low temperature environments is solved, high strength and high toughness are achieved, production process is simplified and reduced cost.
Patent Information
- Application Number
- CN202310319387.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Ductile iron has sharply decreased toughness in low temperature environments, resulting in brittle breakage of parts. The existing production process requires ferrite annealing to improve impact performance, but increases costs and operating cycles.
Using a cast ultra-low temperature ductile iron production method without ferrite annealing, the number of pearlescent systems is controlled and the number of pearlescent systems is simplified by using specific chemical composition and process steps, including the use of silicon magnesium alloy ballastic agents, rare earth ballastic agents and composite inoculants. Process flow to achieve high strength and high toughness.
It realizes cast ultra-low-temperature ductile iron with high impact work at -60℃ without ferrite annealing, simplifies production technology, reduces production energy consumption, and has stable quality, and complies with the QT350-22LT material index.
Smart Images

Figure BDA0004151126270000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting, and mainly relates to a cast ultra-low temperature ductile iron and a production method thereof. Background Art
[0002] When ductile iron is used in low temperature environment, its toughness drops sharply, turning it into a brittle material that cannot withstand the impact of various use environments, which may lead to sudden brittle fracture of parts, thus causing significant economic losses. Improvements in the batching, spheroidization, and inoculation treatment of ductile iron can produce low-temperature high-toughness ductile iron. Low-temperature high-toughness ductile iron is mainly used for important equipment parts in cold regions, such as wind turbine hubs, bases and other components, railway and subway accessories, petroleum and petrochemical accessories, etc.
[0003] With the gradual development of wind farms, areas with harsh environments but rich wind energy resources are also being developed into wind farms, which requires the development of ultra-low temperature ductile iron parts made of QT350-22LT. When the temperature drops to -60°C, the strain rate of impact energy increases significantly with the temperature drop, so there are higher requirements for the pearlite content in the matrix. As far as the existing production process is concerned, the control of pearlite content in the matrix is unstable. In order to meet the material's -60°C impact performance requirements, the casting is generally required to be ferritized annealed to eliminate the pearlite in the casting matrix, which leads to increased costs, longer operating cycles, and reduced labor productivity. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a cast ultra-low temperature ductile iron and a production method thereof, which can produce high-strength and high-toughness ultra-low temperature ductile iron without ferritizing annealing, and the cast material has high impact energy at -60°C.
[0005] In order to achieve the above object, the technical solution of the present invention is as follows:
[0006] A cast ultra-low temperature ductile iron, the chemical components of which are measured by weight percentage, include:
[0007] 3.70% to 3.90% C, 1.90% to 2.10% Si, ≤0.10% Mn, ≤0.030% P, ≤0.012% S, 0.45% to 0.55% Ni, 0.035% to 0.055% Mg, ≤0.006% Ce, ≤0.03% Cu, ≤0.004% Sn, ≤0.0015% Pb, ≤0.001% Bi, ≤0.002% Sb, ≤0.035% Cr, ≤0.002% As, the remainder is Fe and impurity elements; the pearlite number Px of the as-cast ultra-low temperature ductile iron is less than 2.0; the calculation formula of the pearlite number is:
[0008] Px=3.0Mn-2.65(Si-2.0)+7.75Cu+90Sn+357Pb+333Bi+20.1As+9.6Cr+71.7Sb.
[0009] Preferably, the pearlite number Px of the as-cast ultra-low temperature ductile iron is less than 1.7.
[0010] Furthermore, the as-cast ultra-low temperature ductile iron has Rm≥330MPa, Rp 0.2 ≥210MPa, A≥18%; the -60℃ impact absorption energy of the V-notch impact specimen is ≥9J for each value and ≥12J for the average value.
[0011] Furthermore, the spheroidization rate of the as-cast ultra-low temperature ductile iron is ≥90%, and the number of graphites is ≥120 / mm 2 .
[0012] The method for producing any of the above-mentioned as-cast ultra-low temperature ductile iron comprises the following steps:
[0013] Melting: weigh 60% to 70% high-purity pig iron, 30% to 40% low-manganese scrap steel, 0.80% to 1.00% carburizer, and 0.60% to 0.80% ferrosilicon and add them into a melting furnace for melting;
[0014] Pretreatment: adding 0.40% to 0.60% silicon carbide into the smelting furnace;
[0015] Modification treatment, placing 0.40% to 0.50% of silicon-magnesium alloy spheroidizer by weight of the iron, 0.50% to 0.60% of rare earth spheroidizer by weight of the iron, 0.40% to 0.60% of silicon-barium inoculant by weight of the iron, and 0.60% to 0.80% of silicon steel sheet by weight of the iron in a ladle in advance, pouring the pretreated molten iron into the ladle for modification treatment, and slagging after the modification treatment is completed;
[0016] For pouring, a composite inoculant with a pouring weight of 0.1% to 0.15% is placed in the inoculant bucket of the ladle in advance. When pouring, the inoculant flow enters the mold cavity together with the molten iron flow after modification.
[0017] Furthermore, the silicon-magnesium alloy spheroidizer includes 43% to 48% Si, 6.5% to 7.5% Mg and 0.5% to 2.0% Ca.
[0018] Furthermore, the rare earth spheroidizer includes 44% to 48% Si, 5.5% to 6.2% Mg, 0.5% to 1.5% RE and 0.8% to 1.2% Ca.
[0019] Furthermore, the silicon-barium inoculant includes 65% to 75% Si, 2% to 4% Ba and ≤1.5% Ca.
[0020] Furthermore, the composite inoculant comprises 65% to 75% Si, 0.6% to 1.2% Sr, ≤0.10% Ca and ≤0.50% Al.
[0021] Furthermore, in the modification step, the silicon-magnesium alloy spheroidizer and the rare earth spheroidizer are placed in a spheroidization reaction chamber at the bottom of the ladle, the silicon-barium inoculant is placed on the two spheroidizers, and the silicon steel sheet is placed on the silicon-barium inoculant.
[0022] Furthermore, the particle size of the silicon-magnesium alloy spheroidizer is 10 mm to 30 mm, the particle size of the rare earth spheroidizer is 10 mm to 30 mm, the particle size of the silicon-barium inoculant is 1 mm to 6 mm, and the silicon-magnesium alloy spheroidizer, the rare earth spheroidizer, the silicon-barium inoculant and the silicon steel sheet are all compacted.
[0023] Furthermore, the particle size of the composite inoculant is 0.20 mm to 0.80 mm.
[0024] It can be seen from the above technical solution that the advantages and positive effects of the present invention are:
[0025] The as-cast ultra-low temperature ductile iron disclosed in the present invention does not need to be subjected to ferritization annealing, and can meet the material index requirements of QT350-22LT in the as-cast state, has good low-temperature impact toughness at -60°C, simplifies the production process, reduces production energy consumption, and has stable quality.
[0026] The cast ultra-low temperature ductile iron disclosed by the present invention uses a silicon-magnesium alloy spheroidizer and a rare earth spheroidizer for spheroidization treatment, and the spheroidization reaction is stable, the spheroidization rate is high, and the graphite balls have the advantages of high roundness and small graphite balls. Silicon carbide is used for pretreatment, and a composite inoculant is used for instantaneous inoculation during the pouring process, which effectively enhances the nucleation ability of molten iron, prolongs the inoculation effect, refines the grains, promotes the ferritization of the organization, and effectively prevents the generation of pearlite organization. DETAILED DESCRIPTION
[0027] The following specific examples further illustrate the present invention so that those skilled in the art can better understand the present invention and implement it, but the examples are not intended to limit the present invention. According to the common technical knowledge and customary means in this field, without departing from the above-mentioned basic technical concept of the present invention, other various forms of modification, replacement or change made to the above-mentioned structure of the present invention should all fall within the protection scope of the present invention.
[0028] The percentages, % and fractions in the examples are by weight unless otherwise specified.
[0029] The embodiment of the present invention discloses a cast ultra-low temperature ductile iron, wherein the weight percentage of chemical components after furnace casting includes:
[0030] 3.70% to 3.90% C, 1.90% to 2.10% Si, ≤0.10% Mn, ≤0.030% P, ≤0.012% S, 0.45% to 0.55% Ni, 0.035% to 0.055% Mg, ≤0.006% Ce, ≤0.03% Cu, ≤0.004% Sn, ≤0.0015% Pb, ≤0.001% Bi, ≤0.002% Sb, ≤0.035% Cr, ≤0.002% As, the balance is Fe and impurity elements. In order to effectively reduce the pearlite content in the matrix structure, the pearlite number Px of the as-cast ultra-low temperature ductile iron is less than 2.0, wherein the calculation formula of the pearlite number is:
[0031] Px=3.0Mn-2.65(Si-2.0)+7.75Cu+90Sn+357Pb+333Bi+20.1As+9.6Cr+71.7Sb.
[0032] The as-cast ultra-low temperature ductile iron disclosed in the embodiment of the present invention comprises 60% to 70% of high-purity pig iron, 30% to 40% of low-manganese scrap steel, 0.8% to 1.0% of carburizer and 0.6% to 0.8% of ferrosilicon in raw material ratio. High-purity pig iron and low-manganese scrap steel are used in the raw materials to effectively control the pearlite number Px < 2.0, avoid the formation of pearlite structure, and achieve the required -60°C low-temperature impact toughness of the material without ferritizing annealing; the mechanical properties of the material reach Rm ≥ 330MPa, Rp 0.2 ≥210MPa, A≥18%; V-notch impact specimen -60℃ impact absorption energy single value ≥9J, average value ≥12J, metallographic structure reaches spheroidization rate ≥90%, graphite number ≥120 / mm 2 , and no pearlite structure appears in the matrix structure.
[0033] The as-cast ultra-low temperature ductile iron disclosed in the embodiment of the present invention is smelted using an induction furnace, and the smelting process includes:
[0034] Use an electronic scale to weigh 60% to 70% of high-purity pig iron, 30% to 40% of low-manganese scrap steel, 0.8% to 1.0% of carburizer and 0.6% to 0.8% of ferrosilicon, and put them into an induction furnace for melting. The order of adding materials is scrap steel before high-purity pig iron, and the melting temperature is less than 1380°C. After melting, samples can be taken and the composition before the furnace can be detected using a spectrometer. The sampling temperature can be 1420°C to 1440°C, and the overheating temperature can be 1470°C to 1490°C.
[0035] The as-cast ultra-low temperature ductile iron disclosed in the embodiment of the present invention is pre-treated before the furnace after melting, and the pre-treatment process includes:
[0036] 0.40% to 0.60% silicon carbide is added to the induction furnace. Adding silicon carbide for pretreatment can increase the number of eutectic groups and reduce the supercooling of molten iron. Silicon carbide also has a deoxidizing effect, so that the deoxidized product undergoes a series of reactions in the molten iron, reducing the harmful effects of oxides in the rusted furnace charge and effectively purifying the molten iron. Preferably, the particle size of silicon carbide is 1 mm to 4 mm, and the SiC content is ≥ 98%.
[0037] The as-cast ultra-low temperature ductile iron disclosed in the embodiment of the present invention is subjected to a modification treatment after the pretreatment is completed. The modification treatment process includes:
[0038] S1. Put silicon-magnesium alloy spheroidizer and rare earth spheroidizer into the spheroidization reaction chamber at the bottom of the ladle and tamp them, wherein the amount of silicon-magnesium alloy spheroidizer added is 0.40% to 0.50% of the weight of the iron, and the amount of rare earth spheroidizer added is 0.50% to 0.60% of the weight of the iron.
[0039] Silicon magnesium alloy spheroidizer may include 43% to 48% Si, 6.5% to 7.5% Mg and 0.5% to 2.0% Ca, and its particle size may be 10mm to 30mm. Rare earth spheroidizer may include 44% to 48% Si, 5.5% to 6.2% Mg, 0.5% to 1.5% RE and 0.8% to 1.2% Ca, and its particle size may be 10mm to 30mm.
[0040] S2. Place silicon-barium inoculant on the two spheroidizers and tamp them down. The amount of silicon-barium inoculant added is 0.40% to 0.60% of the weight of the iron.
[0041] The silicon-barium inoculant may include 65% to 75% Si, 2% to 4% Ba and ≤1.5% Ca, and its particle size may be 1 mm to 6 mm.
[0042] S3. Cover the silicon-barium inoculant with silicon steel sheets, the amount of silicon steel sheets added is 0.60% to 0.80% of the weight of the iron. The silicon steel sheets are melted when the iron is tapped, which effectively prevents the premature reaction of the molten iron with the inoculant and the spheroidizer, and stabilizes the spheroidization reaction process.
[0043] S4. Transport the ladle to the induction furnace, adjust the ladle to the front of the furnace mouth, tilt the furnace to tap the iron into the ladle, and start the inoculation and spheroidization reaction after the iron tapping. After the spheroidization reaction is completed, remove the slag and take samples to detect the chemical composition after the furnace.
[0044] S5. After the spheroidization reaction is completed, pouring should be completed within 10 minutes to avoid spheroidization inoculation decay.
[0045] It should be noted that before tapping, a composite inoculant needs to be placed in the inoculant bucket of the ladle in advance, and the inoculant bucket is opened during the pouring process so that the composite inoculant in the inoculant bucket flows evenly on the molten iron. The instantaneous inoculation of the composite inoculant can enhance the nucleation ability of the molten iron, prolong the inoculation effect, refine the grains, promote ferritization, and avoid the formation of pearlite to reduce the low-temperature impact toughness of the material.
[0046] The amount of the composite inoculant added can be 0.1% to 0.15% of the pouring weight, the particle size of the composite inoculant can be 0.20 mm to 0.80 mm, and it can be a composite inoculant of strontium, calcium, and barium. Specifically, the composite inoculant can include 65% to 75% Si, 0.6% to 1.2% Sr, ≤0.10% Ca, and ≤0.50% Al.
[0047] The as-cast ultra-low temperature ductile iron disclosed in the embodiment of the present invention can achieve high low-temperature impact toughness while ensuring strength and plasticity without ferritization annealing, simplifying the processing technology, reducing production energy consumption, and having stable quality. The present invention uses a silicon-magnesium alloy spheroidizer in combination with a rare earth spheroidizer for spheroidization, wherein rare earth has a stabilizing spheroidization effect on the molten iron of the hypereutectic composition, can neutralize anti-spheroidizing elements, has strong anti-interference ability, has a large density, a high boiling point, a melting point close to the temperature of the molten iron, and has no boiling and fire smoke during spheroidization; rare earth spheroidizers are used in combination with silicon-magnesium alloy spheroidizers to optimize the kinetic conditions of spheroidization reaction, and have the advantages of stable spheroidization reaction, high spheroidization rate, high roundness of graphite balls, small graphite balls, and uniform distribution.
[0048] The as-cast ultra-low temperature ductile iron disclosed in the embodiment of the present invention was sampled and tested for chemical composition after furnace, and the test results are shown in Table 1. When casting the casting, a U40 cast test block was cast simultaneously, and the mechanical properties and metallographic structure were tested, and the test results are shown in Table 2.
[0049] Table 1 Chemical composition test results (%)
[0050] C Si Mn P S Cu Cr Sn Pb Ce Mg Ni Bi As Sb Test block 1 3.71 1.95 0.09 0.014 0.009 0.030 0.028 0.001 0.001 0.003 0.048 0.46 0.0005 0.0014 0.0012 Test block 2 3.79 1.99 0.08 0.019 0.008 0.026 0.033 0.001 0.001 0.005 0.051 0.51 0.0009 0.0019 0.0005 Test block 3 3.81 2.01 0.09 0.021 0.009 0.022 0.026 0.001 0.001 0.005 0.054 0.49 0.0008 0.0018 0.0007 Test block 4 3.83 2.04 0.08 0.023 0.011 0.026 0.031 0.001 0.001 0.004 0.046 0.50 0.0009 0.0015 0.0005 Test block 5 3.77 2.00 0.08 0.016 0.011 0.029 0.030 0.001 0.001 0.004 0.049 0.54 0.0005 0.0012 0.0005
[0051] Table 2 Mechanical properties and metallographic test results
[0052]
[0053] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A method for producing as-cast ultra-low temperature ductile iron, characterized in that: The chemical composition of the as-cast ultra-low temperature ductile iron comprises, by weight percentage: 3.70%~3.90% C, 1.90%~2.10% Si, ≤0.10% Mn, ≤0.030% P, ≤0.012% S, 0.45%~0.55% Ni, 0.035%~0.055% Mg, ≤0.006% Ce, ≤0.03% Cu, ≤0.004% Sn, ≤0.0015% Pb, ≤0.001% Bi, ≤0.002% Sb, ≤0.035% Cr, ≤0.002% As, the balance is Fe and impurity elements; The pearlite number Px of the as-cast ultra-low temperature ductile iron is less than 2.0; The calculation formula of the pearlite system coefficient is: Px=3.0Mn-2.65(Si-2.0)+7.75Cu+90Sn+357Pb+333Bi+20.1As+9.6Cr+71.7Sb; The production method comprises the following steps: Melting: weigh 60% to 70% high-purity pig iron, 30% to 40% low-manganese scrap steel, 0.80% to 1.00% carburizer, and 0.60% to 0.80% ferrosilicon and add them into a melting furnace for melting; Pretreatment: adding 0.40% to 0.60% silicon carbide into the smelting furnace; Modification treatment, placing 0.40% to 0.50% of silicon-magnesium alloy spheroidizer by weight of the iron, 0.50% to 0.60% of rare earth spheroidizer by weight of the iron, 0.40% to 0.60% of silicon-barium inoculant by weight of the iron, and 0.60% to 0.80% of silicon steel sheet by weight of the iron in a ladle in advance, pouring the pretreated molten iron into the ladle for modification treatment, and slagging after the modification treatment is completed; Pouring: put a composite inoculant with a pouring weight of 0.1% to 0.15% in the inoculant bucket of the ladle in advance. When pouring, open the inoculant bucket, and the inoculant flows into the mold cavity together with the modified molten iron flow; The silicon-magnesium alloy spheroidizer comprises 43% to 48% Si, 6.5% to 7.5% Mg and 0.5% to 2.0% Ca; The rare earth nodulizer comprises 44% to 48% Si, 5.5% to 6.2% Mg, 0.5% to 1.5% RE and 0.8% to 1.2% Ca; The silicon-barium inoculant comprises 65% to 75% Si, 2% to 4% Ba and ≤1.5% Ca; The composite inoculant comprises 65% to 75% Si, 0.6% to 1.2% Sr, ≤0.10% Ca and ≤0.50% Al.
2. The method for producing as-cast ultra-low temperature ductile iron according to claim 1, characterized in that: The as-cast ultra-low temperature ductile iron has Rm≥330MPa, Rp 0.2≥210MPa, and A≥18%; the single value of the -60°C impact absorption energy of the V-notch impact test specimen is ≥9J, and the average value is ≥12J.
3. The method for producing as-cast ultra-low temperature ductile iron according to claim 1, characterized in that: The as-cast ultra-low temperature ductile iron has a spheroidization rate of ≥90% and a number of graphites of ≥120 / mm 2 .
4. The method for producing as-cast ultra-low temperature ductile iron according to claim 1, characterized in that: In the modification step, the silicon-magnesium alloy spheroidizer and the rare earth spheroidizer are placed in the spheroidization reaction chamber at the bottom of the ladle, the silicon-barium inoculant is placed on the two spheroidizers, and the silicon steel sheet is placed on the silicon-barium inoculant.
5. The method for producing as-cast ultra-low temperature ductile iron according to claim 4, characterized in that: The particle size of the silicon-magnesium alloy spheroidizer is 10mm-30mm, the particle size of the rare earth spheroidizer is 10mm-30mm, the particle size of the silicon-barium inoculant is 1mm-6mm, the silicon-magnesium alloy spheroidizer, the rare earth spheroidizer, the silicon-barium inoculant and the silicon steel sheet are all compacted; the particle size of the composite inoculant is 0.20mm-0.80mm.
Citation Information
Patent Citations
Low-temperature tough ferrite nodular cast iron of 60 DEG C below zero and preparation method thereof
CN103436772A
Low-temperature spheroidal graphite cast iron and production technology and application thereof