A 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom and its manufacturing method
By employing specific chemical compositions and heat treatment processes, the problem of insufficient high strength and low-temperature toughness in seamless steel pipes has been solved, resulting in seamless steel pipes with ultra-high strength of 960MPa and good low-temperature toughness. These pipes are suitable for crawler crane booms and possess high strength, low-temperature toughness, and resistance to atmospheric corrosion.
Patent Information
- Application Number
- CN202310309565.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Existing technologies make it difficult to produce seamless steel pipes with a yield strength of 960 MPa or higher, and their low-temperature toughness and weldability are poor, which cannot meet the high strength and high toughness requirements of crawler crane booms.
By employing specific chemical composition design and heat treatment processes, including the combined use of alloying elements such as C, Mn, Cr, Mo, Ni, V, Al, Ti, Nb, and Cu, and by combining normalizing, quenching, high-temperature tempering, and low-temperature tempering treatments, a tempered sorbite + tempered bainite microstructure is formed, the austenite grain size is controlled, and the use of high-cost alloys such as W and Co is avoided.
Seamless steel pipes with ultra-high strength of 960MPa, good low-temperature toughness and atmospheric corrosion resistance are achieved. They are suitable for crawler crane booms, reducing production costs and improving the overall performance of steel pipes.
Smart Images

Figure CN116377324B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of manufacturing low-alloy high-strength seamless steel pipes, and in particular to a 960MPa grade ultra-high-strength and high-toughness seamless steel pipe for a crane boom and a manufacturing method thereof. Background Art
[0002] The mass, volume and lifting height of objects that need to be hoisted in engineering construction are getting larger and larger. Crawler cranes are increasingly showing their superiority due to their flexible mobility and large lifting tonnage. The market capacity has also increased year by year in recent years. In order to meet the needs of the market, manufacturers have made the tonnage of crawler cranes larger and larger, from dozens of tons to the current largest 4,500 tons in China, so higher requirements are put forward for the performance of seamless steel pipes used in the manufacture of crawler crane booms. The use of ultra-high strength and high toughness seamless steel pipes with a yield strength of 960MPa to manufacture crawler crane booms can play an important role in improving equipment efficiency, reducing energy consumption and reducing equipment deadweight. At the same time, it can adapt to the continuous development of crawler cranes towards high parameters, large-scale and lightweight.
[0003] Q960E ultra-high strength steel in the category of low alloy high strength steel belongs to steel used in engineering machinery and offshore platforms. It is currently widely used in plate and strip materials and is a type of steel with high strength level and impact toughness requirements in the plate and strip market. As for the production of seamless steel pipes, products with a yield strength of more than 960MPa are generally made of medium-high carbon alloy steel and low-carbon high alloy steel. The performance is guaranteed by heat treatment processes such as quenching + tempering. The strength of this type of steel can reach a high level, but the low-temperature impact toughness at -40℃ is not good, and the welding performance is not good either. It cannot meet the high strength, high toughness and good welding performance requirements for steel used in engineering machinery. At present, the yield strength level of seamless steel pipes that can be stably produced using low alloy steel can only reach 890MPa.
[0004] Existing high-strength and high-toughness seamless steel pipes for structures are all made by adding appropriate amounts of Cr, Ni, Mo, W, V, Nb, Ti and other alloying elements to low-carbon manganese steel, and then undergoing tempering heat treatment to achieve excellent performance by utilizing the solid solution strengthening of elements such as Mn, Cr, W, Ni, Mo and the precipitation strengthening and fine grain strengthening of micro-alloying elements such as Nb, V, Ti.
[0005] CN201410684446.0 patent discloses a 960MPa grade quenched and tempered steel and its manufacturing method. The invention requires that the yield strength of the product reaches 960MPa and the impact energy at -40℃ is greater than 47J. The patent composition is: C: 0.10%~0.20%, Si: 0.10%~0.50%, Mn: 1.00%~1.60%, P≤0.015%, S≤0.005%, Cr: 0.10%~0.50%, Mo: 0.20%~0.6 0%, V: 0.020%~0.060%, Nb: 0.015%~0.055%, Ti: 0.003%~0.04%, Al: 0.020%~0.070%, B: 0.0006%~0.0025%, the balance is iron and residual elements, CEV≤0.61%; the production process is: the steel billet is subjected to a controlled rolling process to control the final rolling temperature at 820℃~880℃ and then ultra-fast cooling to 500℃~700℃, and finally the performance requirements are achieved through quenching and tempering. The differences of this invention are as follows: This invention is a method for making ultra-high strength steel plates, which adopts a two-stage controlled rolling and controlled cooling method, suitable for the production of 4.0mm~25mm thick steel plates, and this process is not suitable for the production of seamless steel pipes.
[0006] Patent CN202111253774.1 discloses a low yield ratio marine engineering steel plate with a yield strength of 960 MPa and a preparation method thereof. The patented components are: C: 0.10% to 0.20%, Si: 0.10% to 0.30%, Mn: 1.00% to 1.50%, P≤0.010%, S≤0.005%, Cr: 0.20% to 0.60%, Mo: 0.20% to 0.80%, Co: 0.2% to 1.00%, V: 0.020% to 0.100%, Nb: 0 to 0.050%, Ti: 0.005% to 0.015%, Cu: 0 to 0.50%, B: 0.0005% to 0.0020%, and the remainder is iron. The production process is: the steel billet is subjected to controlled rolling and controlled cooling and (α+γ) two-phase annealing + complete austenitization quenching + medium and low temperature treatment to prepare a medium and thick steel plate with high strength, toughness and low yield strength. The differences of this invention are as follows: (1) This invention is a method for making ultra-high strength steel plates, which adopts controlled rolling and controlled cooling methods in the rolling stage. This process is not suitable for the production of seamless steel pipes. (2) Co alloy (0.2% to 1.00%) is added to the composition of this invention, which greatly increases the cost of steel and is not convenient for the production organization of general steel plants.
[0007] The Chinese patent CN202011310801.X is a 960MPa grade ultra-high strength structural steel, steel pipe and its manufacturing method and application. The yield strength of the invented product is required to be greater than or equal to 960MPa, and the impact energy at -40℃ is greater than 45J. Its patented components are: C: 0.12%~0.17%, Si: 0.10%~0.40%, Mn: 0.70%~1.30%, P≤0.010%, S≤0.003%, Cr: 0.50%~1.00%, Mo: 0.70%~1.0%, W: 0.1%~0.3%, Ni: 0.1%~0.4%, Nb: 0.01%~0.06%, Als: 0.01%~0.05%, Ca: 0.0005%~0.005%, and the balance is iron. The continuous casting round billet smelted according to this composition is heated, perforated, rolled, and then quenched + high temperature tempered to ensure that the performance meets the requirements. The difference of this invention is that: (1) W alloy (0.10% to 0.30%) is added to the composition, and the addition amount of Mo alloy (0.70% to 1.0%) is also relatively high, which greatly increases the cost of steel. 2. The microstructure of the steel pipe produced by the process of this invention is a lamellar martensite structure instead of a tempered troostite structure, and does not have the characteristics of ultra-high strength and high low temperature toughness. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide a 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom, which has ultra-high strength, good low-temperature toughness and atmospheric corrosion resistance.
[0009] To achieve the above object, the present invention adopts the following technical solutions:
[0010] The invention discloses a 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom, the chemical composition of which is as follows by weight: C: 0.13%-0.18%, Si: 0.30%-0.50%, Mn: 0.8%-1.00%, P≤0.020%, S≤0.010%, Cr: 0.20%-0.80%, Mo: 0.30%-0.60%, Ni: 0.50%-1.40%, V: 0.030%-0.070%, Al: 0.015%-0.050%, Nb: 0.020%-0.060%, Ti: 0.010%-0.030%, Cu: 0.30%-0.50%, N<0.0060%, and the balance is Fe and unavoidable impurities.
[0011] Ingredients function:
[0012] The main function of C is solid solution strengthening, and it is an important element to ensure the strength of seamless steel pipes. In order to improve hardenability and achieve the requirement of yield strength greater than 960MPa, C must be above 0.12%. However, if C is greater than 0.18%, the plasticity and toughness of the steel will decrease, and a high C content will lead to poor welding performance of the steel. Therefore, the preferred range of C is 0.13% to 0.18%, and the more preferred content range is 0.14% to 0.17%.
[0013] Mn is an austenite stabilizing element and an effective element for improving the toughness of steel. Its influence on the mechanical properties of quenched and tempered steel is mainly achieved by improving the hardenability of steel. If the Mn content is too low, the expected strengthening effect cannot be obtained. If the Mn content is too high, the plasticity and toughness of the steel will decrease. At the same time, a high Mn content will also lead to poor welding performance of the steel. In order to control the carbon equivalent level of the steel, the present invention controls the Mn content to 0.80% to 1.00%, and the more preferred content range is 0.90% to 1.00%.
[0014] Cr can improve the hardenability of steel and increase the strength of steel, but it also tends to increase the temper brittleness of steel, so it should be used in combination with elements such as Mo. Its effect can be clearly manifested when its content is above 0.20%, but if it is added in excess, the plasticity and toughness of the steel will decrease. At the same time, a high Cr content will lead to poor welding performance of the steel, so the preferred range of Cr is 0.20% to 0.80%, and the more preferred content range is 0.40% to 0.60%.
[0015] Mo can improve the hardenability of steel, improve heat resistance, and prevent temper brittleness. The effect is obvious when the Mo content is above 0.20%, but a higher Mo content will lead to poor welding performance of steel, and Mo is a precious metal, so it should be added as little as possible while meeting the performance requirements. Therefore, the preferred range of Mo is 0.30% to 0.60%, and the more preferred content range is 0.35% to 0.50%.
[0016] Ni is the main alloying element for forming and stabilizing austenite, which can significantly improve the low-temperature toughness of steel and achieve high-strength and high-toughness matching of steel. At the same time, Ni can also effectively prevent the hot brittle cracking of Cu-containing steel during hot working. When the Ni content is low, the improvement of the low-temperature toughness of steel is not obvious, especially for thick-walled steel pipes, but too high Ni content will greatly increase the cost of steel. Considering that the yield strength of the product designed by the invention is required to be above 960MPa level, and the low-temperature impact toughness of -40℃ is ≥80J, the preferred range of Ni is 0.50% to 1.40%, and the more preferred content range is 0.80% to 1.40%.
[0017] V plays a major role in precipitation strengthening and fine grain strengthening in low alloy steel, which can increase the strength of the steel and inhibit its aging effect. V content above 0.02% is effective, but when the V content exceeds 0.10%, the toughness of the steel will decrease. Therefore, the preferred range of V is 0.030% to 0.070%, and the more preferred content range is 0.040% to 0.060%.
[0018] Al is the main deoxidizing element in steel and also a cheap grain refining element. The main purpose of adding Al in the present invention is to refine the grains and fix the N in the steel, thereby significantly improving the impact toughness of the steel. The Al content should be greater than 0.015%. If the Al content exceeds 0.05%, it will increase the non-metallic inclusions in the steel or make the toughness worse. Therefore, the upper limit is set to less than 0.050%. The preferred range is 0.015% to 0.05%, and the more preferred content range is 0.020% to 0.040%.
[0019] Ti has a strong affinity with N, O, and C. The present invention adds titanium iron to steel for micro-titanium treatment, utilizes Ti to react with N in the steel to form TiN, and TiN precipitated in a partially solidified state can prevent the growth of grains in the steel pipe during heating, thereby improving the plastic toughness of the steel pipe and the welding performance of the steel pipe. However, excessive addition of Ti is likely to form TiN inclusions, which deteriorates the toughness of the steel pipe, so the range is 0.010% to 0.030%. The preferred range is 0.010% to 0.020%.
[0020] The main role of Nb is precipitation strengthening on the one hand, and on the other hand, it prevents grain growth during austenitization by forming nano-precipitates to pin interface migration. When the Nb content is too low, the precipitation strengthening and grain refinement effects are not obvious, so the lower limit of the Nb content is set to 0.020%, the preferred range is 0.020% to 0.060%, and the more preferred content range is 0.030% to 0.050%.
[0021] Cu can improve the hardenability of steel and is also an important element for improving the atmospheric corrosion resistance of steel. When the Cu content is high, hot brittleness is easily generated during the hot rolling heating process, causing network cracks on the surface of the steel pipe and reducing the toughness of the heat-affected zone of the steel pipe welding. Therefore, its upper limit is set to less than 0.60%, and the preferred range is 0.30% to 0.50%. The present invention can not only improve the strength and -40°C low-temperature toughness of the steel pipe by jointly adding several alloy elements of Cu, Cr and Ni, but also make the steel pipe have atmospheric corrosion resistance.
[0022] P is easy to segregate at grain boundaries, which can increase the ductile-brittle transition temperature and reduce the toughness of steel. Too high a content will lead to a decrease in low-temperature impact toughness of -40°C, so it must be limited to below 0.020%, and the more preferred range should be controlled below 0.015%.
[0023] S is easy to form non-hard inclusions with manganese, etc., and the increase of its content will lead to an increase in the number of inclusions, which will cause extension deformation along the rolling direction during processing, destroy the continuity of the material matrix, and reduce the low-temperature impact toughness of the seamless steel pipe. Therefore, it must be limited to less than 0.010%.
[0024] The influence of N on steel properties is similar to that of carbon and phosphorus. With the increase of nitrogen content, the strength of steel can be significantly improved, but the toughness is significantly reduced and the weldability is deteriorated. In steel microalloyed with Nb, V, Ti and Al, too high N content will form too many nitrides, which will increase the control difficulty during the continuous casting process, increase the probability of cracks on the surface of the continuous casting billet, and eventually cause cracks on the outer surface of the steel pipe, increasing the failure rate of the steel pipe. Therefore, it must be limited to less than 0.0060%, and the more preferred range should be controlled below 0.0050%.
[0025] A method for manufacturing a 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom, the process includes: molten iron pretreatment → converter smelting → LF refining + VD → continuous casting of round tube billets → hot rolled steel pipes → normalizing → quenching + high temperature tempering heat treatment → steel pipe outer surface sandblasting → low temperature tempering → hot straightening → inspection; specifically including:
[0026] 1) After hot rolling, the steel pipe is subjected to normalizing heat treatment at a normalizing temperature of 900°C to 930°C, and then air-cooled, wind-cooled or mist-cooled after being kept at this temperature for 30 to 50 minutes;
[0027] 2) After normalizing heat treatment, the steel pipe is subjected to quenching + high temperature tempering heat treatment. The steel pipe is heated at 890℃~910℃ in a heating furnace and kept warm for 30~40 minutes before external showering + internal water spraying quenching. Then, it is heated at 600℃~650℃ in a tempering furnace and kept warm for 45~90 minutes before air cooling.
[0028] 3) After high temperature tempering, the outer surface of the steel pipe is sandblasted to remove the iron oxide attached to the outer surface of the steel pipe;
[0029] 4) After sandblasting, the steel pipe is subjected to low-temperature tempering heat treatment: the steel pipe is heated at 500℃~550℃ in a tempering furnace and kept warm for 20~30 minutes before being straightened with temperature to ensure that the curvature of the steel pipe per meter is no more than 1.2mm and the curvature of the entire length is no more than 1‰.
[0030] The diameter of the round tube billet in the continuous casting round tube billet process is 200-220 mm.
[0031] In the hot-rolled steel pipe process, the heating temperature of the round tube billet is 1240℃~1270℃, and after heating, it is pierced, rolled by a continuous tube mill, and sizing by a sizing mill. After rolling, the outer diameter of the steel pipe is 101.6~180mm and the wall thickness is 10~25mm.
[0032] The average cooling rate during the water quenching treatment in step 2) is above 40°C / second.
[0033] A 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom, mechanical properties: yield strength: Rp 0.2 ≥960MPa; tensile strength: R M 980~1200MPa; Elongation: A≥14%; -40℃ average impact absorption energy KV2: ≥80J.
[0034] The structure of the steel pipe is tempered bainite + ≤10% tempered bainite, and the austenite grain size is ≥10 grades.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The composition design takes economic considerations into account, avoiding the addition of expensive alloys such as W and Co, and instead considering adding appropriate amounts of Cr, Mo, and Ni alloys for solid solution strengthening; and using V, Nb, and Al for microalloying to achieve the purpose of precipitation strengthening and grain refinement; special consideration is given to adding Ti, which can effectively prevent the growth of austenite grains under high temperature conditions of hot rolling, and play a role in refining austenite grains from the root; the combined effect of adding appropriate amounts of Cu, Cr, and Ni alloy elements makes the product's atmospheric corrosion resistance significantly higher than similar products without Cu alloys, and improves the paintability of the steel pipe surface. At the same time, controlling N in the steel to less than 0.0060% can effectively reduce the crack defects on the surface of the continuous casting billet. Under this composition, the strength and low-temperature toughness indicators of the seamless steel pipe are guaranteed to meet the requirements by performing a special heat treatment process on the steel pipe.
[0037] (2) Seamless steel pipes treated by normalizing + quenching + high temperature tempering have a microstructure of tempered bainite + ≤10% tempered bainite, and an austenite grain size of ≥10. They have the characteristics of high strength and low temperature toughness. This heat treatment process is especially beneficial for the production of thick-walled pipes with a wall thickness of more than 20 mm.
[0038] (3) After the steel pipe is tempered, the outer surface is sandblasted, and then heated and straightened at 500℃~550℃. This can effectively avoid the defects of pitting and pitting on the outer surface of the steel pipe after straightening, and ensure that the curvature of the steel pipe per meter is not more than 1.2mm, and the curvature of the entire length is not more than 1‰.
[0039] (4) The performance of the low alloy ultra-high strength seamless steel pipe for crane boom manufactured by the present invention can meet the following requirements: yield strength Rp 0.2 ≥960Mpa, tensile strength R M 980~1200Mpa, elongation after fracture A≥14%, -40℃ low temperature impact toughness KV2≥80J. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is the metallographic structure diagram of tempered bainite + 8% tempered bainite in Example 6.
[0041] Figure 2 This is a schematic diagram of the austenite grain size level 11 in Example 6.
[0042] Figure 3 Comparison of AC impedance results between Example 5 and Comparative Example 1.
[0043] Figure 4 Comparison of potentiodynamic polarization results of Example 5 and Comparative Example 1. DETAILED DESCRIPTION
[0044] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] The invention discloses a 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom, the chemical composition of which is as follows by weight: C: 0.13%-0.18%, Si: 0.30%-0.50%, Mn: 0.8%-1.00%, P≤0.020%, S≤0.010%, Cr: 0.20%-0.80%, Mo: 0.30%-0.60%, Ni: 0.50%-1.40%, V: 0.030%-0.070%, Al: 0.015%-0.050%, Nb: 0.020%-0.060%, Ti: 0.010%-0.030%, Cu: 0.30%-0.50%, N<0.0060%, and the balance is Fe and unavoidable impurities.
[0046] A method for manufacturing a 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom, the process includes: molten iron pretreatment → converter smelting → LF refining + VD → continuous casting of round tube billets → hot rolled steel pipes → normalizing → quenching + high temperature tempering heat treatment → steel pipe outer surface sandblasting → low temperature tempering → hot straightening → inspection; specifically including:
[0047] (1) Converter smelting, LF refining + VD, continuous casting round billet diameter is 200-220mm;
[0048] (2) The continuously cast round billet is rolled into a steel pipe with an outer diameter of 101.1 to 180 mm and a wall thickness of 10 to 25 mm by a steel pipe continuous rolling mill. The heating temperature of the round billet is 1240°C to 1270°C. After heating, it is pierced, rolled by a continuous tube mill, and sized by a sizing mill.
[0049] (3) After hot rolling, the steel pipe is subjected to normalizing heat treatment at a temperature of 900°C to 930°C. After keeping the temperature for 30 to 50 minutes, it is air-cooled, wind-cooled or mist-cooled. This is a preliminary heat treatment process, the purpose of which is to refine the grains and make the structure uniform, so as to provide a good basic structure for the subsequent quenching and tempering treatment.
[0050] (4) After normalizing, the steel pipe is subjected to quenching + high temperature tempering heat treatment. The steel pipe is heated in a heating furnace at 890℃~910℃ and kept warm for 30~40 minutes, and then subjected to external showering + internal spraying quenching. The main purpose of quenching is to quench all the austenitized steel pipe into martensite, so that good microstructure and mechanical properties can be obtained after tempering at an appropriate temperature. The quenching temperature range is designed to be 890℃~910℃ based on the phase transition point temperature AC3 (860℃~870℃) measured for the invented steel grade. To ensure that the steel pipe achieves high strength and high toughness matching, sufficient cooling intensity must be achieved during water quenching, and the average cooling rate during water quenching is above 40℃ / second.
[0051] Then, the steel pipe is heated at 600℃~650℃ and kept at this temperature for 45~90 minutes in a tempering furnace, and then air-cooled for tempering heat treatment; the residual stress after quenching of the steel pipe is eliminated, and the plasticity and toughness of the steel are increased. After normalizing + quenching + high temperature tempering, the austenite grain size of the seamless steel pipe is ≥10 grades. The microstructure is tempered bainite + ≤10% of a small amount of tempered bainite.
[0052] (5) The outer surface of the tempered steel pipe is sandblasted to remove the iron oxide attached to the outer surface of the steel pipe; to avoid the formation of pitting or pitting defects on the outer surface of the steel pipe after straightening.
[0053] (6) After sandblasting, the steel pipe is subjected to low-temperature tempering. The steel pipe is heated at 500℃~550℃ in the tempering furnace and kept warm for 20~30 minutes before being straightened with heat to ensure that the curvature of the steel pipe per meter is no more than 1.2mm and the curvature of the entire length is no more than 1‰.
[0054] The ingredients of the embodiments and comparative examples (comparative examples contain W) are shown in Table 1.
[0055] Table 1 Composition of steel in the embodiments of the present invention and comparative examples (wt%)
[0056]
[0057] The main performance indicators of the embodiments and comparative examples under heat treatment are shown in Table 2.
[0058] Table 2 Mechanical properties and austenite grain size
[0059]
[0060]
[0061] Electrochemical tests have shown that the steel designed in the present invention has better atmospheric corrosion resistance than similar steel without Cu alloy. Figure 1 and Figure 2 The test results show that the arc radius of the capacitance of the Cu-containing alloy in Example 5 (31#) designed by the present invention is larger than that of the comparative example 1 (13#) of the similar Cu-free alloy. Combined with the potentiodynamic polarization, it can be seen that the atmospheric corrosion resistance of the Cu-containing alloy in Example 5 (31#) designed by the present invention is better. Figure 3-Figure 4 .
[0062] The present invention can be used on the main rotating tube of the crawler crane boom and various high-strength structural parts, and can also provide the required seamless steel pipes for various projects such as engineering machinery structural parts, grid structures, marine engineering, bridges, etc.
[0063] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for manufacturing a 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom, characterized in that: The chemical composition of the 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom is as follows by weight percentage: C: 0.13%~0.18%, Si: 0.30%~0.50%, Mn: 0.8%~0.88%, P≤0.020%, S≤0.010%, Cr: 0.20%~0.80%, Mo: 0.30%~0.60%, Ni: 0.50%~0.87%, V: 0.030%~0.070%, Al: 0.015%~0.050%, Nb: 0.020%~0.060%, Ti: 0.010%~0.030%, Cu: 0.36%~0.50%, N<0.0060%, the balance is Fe and unavoidable impurities; the microstructure is tempered troostite + ≤10% tempered bainite; the austenite grain size is ≥10 grades; the phase transition temperature AC3: 860℃~870℃; Mechanical properties: Yield strength: Rp0.2≥1010MPa; Tensile strength: RM 1040~1200MPa; Elongation: A≥14%; Average impact absorption energy at -40℃ KV2≥80J; The manufacturing process is: hot metal pretreatment → converter smelting → LF refining + VD → continuous casting / continuous rolling round tube billet → hot rolled steel pipe → normalizing → quenching + high temperature tempering heat treatment → steel pipe outer surface sandblasting → low temperature tempering → hot straightening → inspection; specifically includes: 1) In the hot-rolled steel pipe process, the heating temperature of the round tube billet is 1240℃~1270℃. After heating, it is pierced, rolled by a continuous tube mill, and sized by a sizing mill. After rolling, the outer diameter of the steel pipe is 101.1~180mm and the wall thickness is 10~25mm. After hot rolling, the steel pipe is subjected to normalizing heat treatment: the normalizing temperature is 900℃~930℃, and it is kept warm for 30~50 minutes before being air-cooled or mist-cooled. 2) After normalizing heat treatment, the steel pipe is subjected to quenching + high temperature tempering heat treatment: the steel pipe is heated at 890℃~910℃ in a heating furnace, and kept warm for 30~40 minutes before external showering + internal spraying quenching. The average cooling rate during water quenching is more than 40℃ / second. The purpose of quenching is to quench all austenitized steel pipes into martensite, and then heated at 600℃~650℃ in a tempering furnace, kept warm for 45~90 minutes, and then air-cooled; 3) After high temperature tempering, the outer surface of the steel pipe is sandblasted to remove the iron oxide attached to the outer surface of the steel pipe; 4) After sandblasting, the steel pipe is subjected to low-temperature tempering heat treatment: the steel pipe is heated at 500℃~550℃ in the tempering furnace and After 20 to 30 minutes of heat preservation, hot straightening is carried out to ensure that the curvature of the steel pipe per meter is no more than 1.2 mm and the curvature of the entire length is no more than 1‰.
2. The method for manufacturing a 960MPa grade ultra-high strength and high toughness seamless steel pipe for crane boom according to claim 1, characterized in that: The diameter of the round tube billet in the continuous casting / continuous rolling round tube billet process is 200-220 mm.
Citation Information
Cited By
Low-temperature high-toughness hot continuous rolling thin steel plate with yield strength of 960 MPa or above and production method
CN120099431A