A Cr2AlC-Fe based conductive wear-resistant coating and preparation method thereof

Through the preparation of Cr2AlC-Fe-based composite coating, the problems of wear and arc ablation of steel-aluminum composite contact rails during electrical contact are solved, high hardness and wear-resistant self-lubricating properties are achieved, and the service life of the contact rails is extended and Maintenance costs are reduced.

CN116377369BActive Publication Date: 2024-10-22BEIJING JIAOTONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310262234.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-14
Publication Date
2024-10-22
Estimated Expiration
2043-03-14

AI Technical Summary

Technical Problem

The steel-aluminum composite contact rail has a high wear rate during the electrical contact process, and the contact rail elbows are prone to arc ablation, which affects the service life and operation stability. The existing technology mainly relies on replacement, resulting in high maintenance costs.

Method used

Cr2AlC-Fe-based composite coating is used. By adjusting the Cr2AlC content and using atmospheric supersonic plasma spraying process, a composite coating with high hardness and wear-resistant self-lubricating properties is prepared. It is combined with Fe-based alloy powder for ball milling and spraying to form High hardness and wear-resistant conductive coating.

Benefits of technology

The microhardness is 400-600HV and the tensile interface bonding strength is 30-35MPa, which extends the service life of the contact rail, reduces maintenance costs, improves wear resistance and ablation resistance, and significantly reduces the wear and maintenance costs of the contact rail.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116377369B_ABST
    Figure CN116377369B_ABST
Patent Text Reader

Abstract

The present invention relates to a Cr2AlC-Fe-based conductive wear-resistant composite coating and a preparation method thereof. The chemical composition mass percentage of the composite coating of the present invention is: Cr2AlC: 5-15%, CrC: 0.1-1%, Al2O3: 1-5%, and the rest is Fe-based alloy, and the sum of each component is 100%. The chemical composition mass percentage of the raw material powder of the composite coating is: Cr2AlC: 5-20%, and the rest is Fe alloy powder, and the sum of the two components is 100%. In addition, the particle size of the raw material powder of the composite coating is: Fe alloy powder; 15-45μm, Cr2AlC: 15-40μm. Preparation method: weigh Cr2AlC and Fe alloy raw material powders in the required ratio; place the raw material powders in a planetary ball mill and mix them thoroughly; wash, dry and sandblast the Fe-based alloy substrate, place it in a muffle furnace and preheat it to 100°C and keep it warm for 5 minutes; place the composite raw material powder in the powder feeder of the supersonic plasma spraying equipment, fix the preheated Fe-based alloy substrate on the supersonic plasma spraying equipment with a clamp, select appropriate plasma spraying parameters, and perform supersonic plasma spraying preparation to finally obtain a conductive and wear-resistant composite coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a Cr2AlC-Fe based conductive wear-resistant coating and a preparation method thereof. Background Art

[0002] Urban rail transit has unique advantages such as economy, environmental protection, and high efficiency, and plays a positive role in improving transportation capacity and improving the travel efficiency of the masses. my country's urban rail transit is mainly driven by electricity, so higher requirements are placed on the stability and life of the power supply. The power supply methods currently used are mostly contact network and contact rail power supply. Its steel-aluminum composite contact rail has the advantages of good conductivity, high safety factor, low maintenance cost, good wear resistance, long power supply distance, small engineering earthwork volume, and good urban landscape. It has become the leading direction of urban rail development. It has been widely used in urban rail transit in Guangzhou, Beijing and other cities (Reference: Liu Weiqiang, Railway Standard Design, 2007, [79-82]: 10).

[0003] The steel-aluminum composite contact rail uses aluminum as the current carrier and stainless steel as the contact material. On the one hand, it ensures the high conductivity required by the guide rail, and on the other hand, it satisfies the wear and corrosion resistance of the contact surface friction pair. Among them, the contact rail elbow is an important device for contact rail power supply. It plays a key role in ensuring that the current collector system passes through the broken rail smoothly and guides the collector shoe to go up and down the line smoothly (reference: Wang Wenjuan, Journal of East China Jiaotong University, 2014, [34-38]: 31). However, due to the electrical contact characteristics of the collector shoe and the power supply rail, the contact rail is in a current-carrying friction state for a long time. In this state, the resistance heat participates in the movement of the friction pair, making the friction conditions more severe, which leads to a higher wear rate of the contact rail. At the same time, due to the working characteristics of the contact rail elbow, arc erosion often occurs near the end elbow, affecting the surface morphology of the contact rail elbow and thus affecting the running stability and service life of the contact rail (reference: Chen Xiang, Science and Technology Wind, 2016, [3-4]: 14). At present, my country mostly adopts the method of directly replacing the contact rail after the wear rate exceeds the standard or the ablation is so serious that it does not meet the use standard. This method is simple and direct, but as my country's urban rail transit system continues to grow, it has become a considerable maintenance cost. Therefore, it is extremely important to use coating to enhance the wear resistance and ablation resistance of the elbow.

[0004] Among many material systems, Fe alloy is the most widely used material at present. It has the characteristics of low cost, excellent performance and controllable performance. At the same time, since it is a homogeneous material with steel strip, using this material as the main body of the coating can ensure that the coating is tightly bonded on the one hand, and the electrical properties are similar on the other hand, without affecting its original conductivity. On the other hand, by adjusting the composition, the surface wear resistance and corrosion resistance can be improved, and it has flexible controllability. However, it is difficult for a simple Fe-based coating to improve the surface wear resistance and contact conditions. Therefore, it is necessary to add ceramics to form a composite material to improve its friction and wear performance. The new ternary layered MAX phase ceramic is a good damage tolerance ceramic material with high strength and high toughness and excellent conductivity of metal-like materials (reference: MWBarsoum et al., Progress in Solid State Chemistry, 2000, [201-281]: 28). Typical materials include Ti3SiC2, Ti2AlC, Ti3(SiAl)C2 solid solution and Cr2AlB2, with a density of 4-5g / cm 3 , Young's modulus is 280-340GPa, and room temperature fracture toughness is 6.0-7.88MPa·m 1 / 2 (Reference: MW Barsoum et al., American Scientist, 2001, [336-345]; 89). In addition, the new ternary MAX phase ceramic has excellent wear resistance and self-lubricating properties, and also has the comprehensive advantage of good wetting and bonding with the metal matrix. Therefore, the control of Cr2AlC content and atmospheric supersonic plasma spraying process become the key points of this patent. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a wear-resistant conductive coating using high-hardness and high-wear-resistant ternary layered ceramic Cr2AlC and Fe-based alloy powder as raw materials.

[0006] The Cr2AlC-Fe based composite coating of the present invention has the following components:

[0007] A Cr2AlC-Fe based composite coating and a preparation method thereof, characterized in that the chemical composition mass percentage of the composite coating is: Cr2AlC: 5-15%, CrC: 0.1-1%, Al2O3: 1-5% and the rest is Fe based alloy, and the sum of the components is 100%.

[0008] The raw material powder composition of the Cr2AlC-Fe based composite coating of the present invention is as follows:

[0009] The chemical composition mass percentage of the composite coating raw material powder is: Cr2AlC: 5-20%, the rest is Fe alloy powder, and the sum of the two components is 100%. In addition, the particle size of the composite coating raw material powder is: Fe alloy powder; 15-45μm, Cr2AlC: 15-40μm.

[0010] The mechanical properties of the Cr2AlC-Fe based composite coating of the present invention are as follows:

[0011] The microhardness of the composite coating is 400-600 HV, and the tensile interface bonding strength of the composite coating is 30-35 MPa.

[0012] The present invention has the following beneficial effects:

[0013] The invention can be used as a functional layer on the surface of a subway contact rail to improve the friction performance of the contact rail surface. The wear-resistant self-lubricating property of the invention can extend the service life of the contact rail, reduce its maintenance cost, and has considerable economic benefits.

[0014] The preparation method of the present invention comprises the following steps:

[0015] Step 1, preparing the composite coating raw material powder according to the ratio and particle size described in claim 2, including Cr2AlC and Fe alloy raw material powders, both of which are commercial powders, and placing the above two raw material powders in a planetary ball mill for 6-8 hours to achieve sufficient mixing;

[0016] Step 2, the composite coating of claim 1 uses an Fe-based alloy as a substrate, the substrate is degreased with acetone, and the surface is activated by sandblasting, and the substrate is placed in a muffle furnace and preheated to 100° C. and kept warm for 5 minutes;

[0017] Step 3, the powder of claim 2 should be dried at 70°C before use, and the drying time should be not less than 30 minutes;

[0018] Step 4, placing the composite raw material powder according to claim 2 on the powder feeder of the supersonic plasma spraying equipment, fixing the preheated Fe-based alloy substrate on the supersonic plasma spraying equipment with a clamp, and then preparing the composite coating by atmospheric supersonic plasma spraying, and the specific spraying parameters are as follows: argon gas flow rate 110-130L / min, hydrogen gas flow rate 10-20L / min, voltage 100-120V, current 350-450A, powder feeding pressure 0.4-0.5MPa, powder feeding flow rate 18-20g / min, spraying distance 100-150mm;

[0019] Step 5: The thickness of the composite coating finally obtained is 0.5 to 2 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1: Scanning electron microscopy image of 10wt.%Cr2AlC / 90wt.%410 stainless steel composite coating.

[0021] Figure 2: Scanning electron microscopy image of 12wt.%Cr2AlC / 88wt.%410 stainless steel composite coating.

[0022] Figure 3: Scanning electron microscopy image of 15wt.%Cr2AlC / 85wt.%410 stainless steel composite coating. DETAILED DESCRIPTION

[0023] The present invention provides a Cr2AlC-Fe based composite coating and a preparation method thereof. The present invention is described in detail below with reference to the accompanying drawings and embodiments, but the present invention is not limited thereto.

[0024] Example 1

[0025] According to the mass percentage of the raw material powder of the composite coating: Cr2AlC: 10%, 410 stainless steel powder: 90%, the sum of the two components is 100%, and the required powder is weighed; the above two raw material powders are placed in a planetary ball mill for 8 hours to achieve full mixing; the Fe-based alloy substrate is cleaned with acetone and the surface is sandblasted, and then placed in a muffle furnace to be preheated to 100°C and kept warm for 5 minutes; the above mixed powder is dried for 30 minutes and then placed in a powder feeder of a supersonic plasma spraying equipment, and the preheated Fe-based alloy substrate is fixed on the supersonic plasma spraying equipment with a clamp, and according to the plasma spraying parameter range described in claim 4, appropriate plasma spraying parameters are selected, and then supersonic plasma spraying is performed to finally obtain a composite coating, as shown in Figure 1.

[0026] Example 2

[0027] According to the mass percentage of the raw material powder of the composite coating: Cr2AlC: 12%, 410 stainless steel powder: 88%, the sum of the two components is 100%, weigh the required powder; place the above two raw material powders in a planetary ball mill for 8 hours to achieve full mixing; after the Fe-based alloy substrate is cleaned with acetone and the surface is sandblasted, it is placed in a muffle furnace and preheated to 100°C and kept warm for 5 minutes; after the above mixed powder is dried for 30 minutes, it is placed in the powder feeder of the supersonic plasma spraying equipment, and the preheated Fe-based alloy substrate is fixed on the supersonic plasma spraying equipment with a clamp, and according to the plasma spraying parameter range described in claim 4, appropriate plasma spraying parameters are selected, and then supersonic plasma spraying is performed to finally obtain a composite coating, as shown in Figure 2.

[0028] Example 3

[0029] According to the mass percentage of the raw material powder of the composite coating: Cr2AlC: 15%, 410 stainless steel powder: 85%, the sum of the two components is 100%, and the required powder is weighed; the above two raw material powders are placed in a planetary ball mill for 8 hours to achieve full mixing; the Fe-based alloy substrate is cleaned with acetone and the surface is sandblasted, and then placed in a muffle furnace to be preheated to 100°C and kept warm for 5 minutes; the above mixed powder is dried for 30 minutes and then placed in a powder feeder of a supersonic plasma spraying equipment, and the preheated Fe-based alloy substrate is fixed on the supersonic plasma spraying equipment with a clamp, and according to the plasma spraying parameter range described in claim 4, appropriate plasma spraying parameters are selected, and then supersonic plasma spraying is performed to finally obtain a composite coating, as shown in Figure 3.

Claims

1. A Cr 2 Preparation method of AlC-Fe based conductive wear-resistant composite coating, It is characterized in that The method comprises the following steps: Step 1, Cr 2 The chemical composition mass percentage of the raw material powder used in the AlC-Fe based conductive wear-resistant composite coating is: Cr 2 AlC: 5-20%, the rest is Fe alloy powder, and the powders are all commercial powders; the two raw material powders are placed in a planetary ball mill and ball milled for 6-8 hours to achieve full mixing; Step 2, Cr 2 The AlC-Fe based conductive wear-resistant composite coating uses Fe based alloy as the substrate. The substrate is degreased with acetone and treated with sand blasting for surface activation. The substrate is placed in a muffle furnace and preheated to 100 °C and kept warm for 5 min. Step 3, the Cr 2 AlC powder and Fe alloy raw material powder should be dried at 70 ℃ before use, and the drying time should not be less than 30 min; Step 4, placing the composite raw material powder on the powder feeder of the supersonic plasma spraying equipment, fixing the preheated Fe-based alloy substrate on the supersonic plasma spraying equipment with a clamp, and then preparing the composite coating by atmospheric supersonic plasma spraying. The specific spraying parameters are as follows: argon gas flow rate 110~130 L / min, hydrogen gas flow rate 10~20 L / min, voltage 100~120V, current 350~450 A, powder feeding pressure 0.4~0.5 MPa, powder feeding flow rate 18~20 g / min, spraying distance 100~150 mm; Step 5: The thickness of the composite coating finally obtained is 0.5~2 mm, and the mass percentage of the chemical composition in the composite coating is Cr 2 AlC: 5-15%, CrC: 0.1-1%, Al 2 O 3 : 1-5%, the rest is Fe-based alloy, and the sum of all components is 100%.

2. The Cr according to claim 1 2 Preparation method of AlC-Fe based conductive wear-resistant composite coating, It is characterized in that The particle sizes of raw material powders are: Fe alloy powder; 15-45 μm, Cr 2 AlC: 15-40 μm.

3. The Cr according to claim 1 2 Preparation method of AlC-Fe based conductive wear-resistant composite coating, It is characterized in that The microhardness of the composite coating is 400-600 HV, and the tensile interface bonding strength of the composite coating is 30-35 MPa.

4. Cr prepared by the preparation method according to claim 1 2 AlC-Fe based conductive wear-resistant composite coating, It is characterized in that The mass percentage of chemical composition in the composite coating is: Cr 2 AlC: 5-15%, CrC: 0.1-1%, Al 2 O 3 : 1-5%, the rest is Fe-based alloy, and the sum of all components is 100%.

Citation Information

Patent Citations

  • Novel CeO2 modified iron-base alloy abrasion-resistant coating and preparation method

    CN110184556A

  • Preparation method of MAX phase-based coating

    CN111690892A

  • Preparation method of iron-based coating and preparation method and device of workpiece

    CN114293130A

  • Nickel molybdenum aluminium ( nimoal) chromium aluminium carbide (cr2alc) max phase composite coatings for automotive applications and a method for making the same

    IN202141017480A

  • Plasma sprayed oxygen transport membrane

    JP2003253417A