A kind of fluorinated graphene insulating thermal conductive film and preparation method thereof
The method for preparing fluorinated graphene insulating and thermally conductive films without the addition of a second-phase matrix, by combining pre-expansion and foaming treatment with gas-phase fluorination process, solves the problem of poor thermal conductivity of fluorinated graphene materials, and achieves improved high thermal conductivity and insulation performance, making it suitable for industrial production.
Patent Information
- Application Number
- CN202310480247.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing fluorinated graphene materials have poor thermal conductivity and suffer from problems such as high interfacial thermal resistance, high spatial thermal resistance, and poor mechanical properties.
A method for preparing fluorinated graphene insulating and thermally conductive films without the addition of a second-phase matrix is adopted. Graphene oxide films are prepared by the Hummers method, followed by pre-expansion and foaming treatment, and combined with a gas-phase fluorination process, including intermittent vacuum treatment, to prepare fluorinated graphene insulating and thermally conductive films with high thermal conductivity and volume resistivity.
It significantly reduces the thermal resistance of the thin film phase interface, increases the thermal conductivity to 550-800 W·(m·k)-1, and the volume resistivity is 1-10×1013 Ω·cm, achieving high-efficiency insulation and thermal conductivity, making it suitable for industrial-scale production.
Smart Images

Figure CN116377710B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of graphene material preparation, and in particular relates to a fluorinated graphene insulating thermal conductive film and a preparation method thereof. Background Art
[0002] With the rapid development of informatization and intelligence, electronic and electrical devices are becoming increasingly miniaturized, high-performance, and integrated, with higher power density and more serious heat generation. The generation and retention of heat will exponentially affect the life and stability of devices.
[0003] Graphene, a nanostructured carbon atom 2 The honeycomb two-dimensional carbon material formed by hybridization has become a star material in the 21st century due to its series of excellent physical and chemical properties since its preparation in 2004, including up to 5300W.(mk) -1 The thermal conductivity of graphene makes it widely used in the field of device heat dissipation, with significant effects. In addition, graphene also has excellent electrical conductivity, with an electrical conductivity of up to 5.98×10 4 sm -1 However, there are some application scenarios that require not only excellent heat dissipation performance but also excellent insulation performance. Obviously, we have to find a high thermal conductivity insulation material.
[0004] Fluorinated graphene is a graphene derivative in which fluorine atoms are mainly bonded to carbon atoms by covalent bonds to form CF. Studies have shown that with the continuous introduction of fluorine atoms, the proportion of insulating CF covalent bonds increases, and the intrinsic C=C sp 2 Hybridization will gradually transform into CF sp 3 Hybridization, conductivity decreases, when the F / C ratio is greater than 1, graphene becomes an insulator. It not only has excellent insulation properties, but also has excellent thermal conductivity and thermal stability. Theory shows that after 100% fluorination, fluorinated graphene can still maintain 35% of the initial thermal conductivity, that is, 1800W. (mk) -1 , is an ideal insulating and heat dissipating material.
[0005] At present, the preparation of fluorinated graphene thermal conductive materials can be mainly divided into three types. One is to use fluorinated graphene powder as raw material, add PVA, PVDF and other adhesives to filter and form a film (CN109912912A A flexible, electrically insulating fluorinated graphene thermal conductive composite film and its preparation and application), with a thermal conductivity of 50-60W. (mk) -1 The second method is to add fluorinated graphene powder to EVA, PC, PI and other matrices for physical mixing to form a film (CN113321444A A fluorinated graphene thermal conductive film and its preparation method and application), with a thermal conductivity of 50-60W. (mk)-1 The third method is to dissolve the fluorinated graphene in a solvent and then vacuum press it into a film (CN115231565A fluorinated graphene thermal conductive film and its preparation method), with a thermal conductivity of 250-500W. (mk) -1 The films prepared by these three methods usually have large interfacial thermal resistance and spatial thermal resistance, which will accelerate phonon scattering and inhibit the heat transfer and heat dissipation process. Moreover, under the adhesive addition strategy and matrix composite strategy, the loading amount of fluorinated graphene is low, the heat dissipation and thermal conductivity are not good, and the overall mechanical properties of the film are poor.
[0006] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0007] The purpose of the present invention is to solve the problem that the current fluorinated graphene material has poor thermal conductivity, and to provide a fluorinated graphene insulating thermal conductive film with a higher thermal conductivity coefficient and a preparation method thereof.
[0008] The first aspect of the present invention provides a fluorinated graphene insulating thermally conductive film, wherein no second phase matrix is added to the fluorinated graphene insulating thermally conductive film, and the numerical ranges of the thermal conductivity and volume resistivity of the fluorinated graphene insulating thermally conductive film are as follows:
[0009] Thermal conductivity is 550-800W·(m·k) -1 (including 550W·(m·k) -1 ), and the volume resistivity is 1-10×10 13 Ω·cm;
[0010] Or thermal conductivity is 400-550W·(m·k) -1 (Excluding 550W·(m·k) -1 ), and the volume resistivity is greater than 10 14 Ω·cm.
[0011] A second aspect of the present invention provides a method for preparing a fluorinated graphene insulating thermally conductive film, comprising the following steps:
[0012] (1) preparing a graphene oxide film;
[0013] (2) pre-expanding the graphene oxide film;
[0014] (3) performing foaming treatment on the film that has undergone the pre-expansion treatment;
[0015] (4) subjecting the foamed film to carbonization and graphitization;
[0016] (5) performing a fluorination treatment on the film that has been subjected to the carbonization treatment and the graphitization treatment to obtain a fluorinated graphene film;
[0017] (6) The fluorinated graphene film is rolled to form the fluorinated graphene insulating thermal conductive film.
[0018] In one embodiment of the present invention, the graphene oxide film in step (1) is obtained by preparing graphene oxide slurry by Hummers method, and then coating the slurry and drying it.
[0019] In one embodiment of the present invention, the coating film has a thickness of 1-1.5 cm.
[0020] In one embodiment of the present invention, the coating film has a thickness of 1.1-1.3 cm.
[0021] In one embodiment of the present invention, the thickness of the coating film is 1.2 cm.
[0022] In one embodiment of the present invention, the reagents used in preparing graphene oxide by the Hummers method mainly include flake graphite, potassium permanganate and concentrated sulfuric acid.
[0023] In one embodiment of the present invention, the mesh size of the flake graphite is 50-2000 mesh.
[0024] In one embodiment of the present invention, the mesh size of the flake graphite is 100-300 meshes.
[0025] In one embodiment of the present invention, the ratio of the flake graphite to potassium permanganate and concentrated sulfuric acid is 1:4-10 and 1:20-40 respectively.
[0026] In one embodiment of the present invention, the ratios of the flake graphite to potassium permanganate and concentrated sulfuric acid are 1:6 and 1:35 respectively.
[0027] In one embodiment of the present invention, the slurry needs to be washed by filter pressing 5 times to remove the reaction solution.
[0028] In one embodiment of the present invention, the mass percentage of the solid content of the slurry is 3%-5%.
[0029] In one embodiment of the present invention, the mass percentage of the solid content of the slurry is 4%.
[0030] In one embodiment of the present invention, the slurry is coated on a fiber filter cloth, shaped and dried to obtain the graphene oxide film.
[0031] In one embodiment of the present invention, the coating film drying temperature is 60-100°C.
[0032] In one embodiment of the present invention, the coating film drying temperature is 90°C.
[0033] In one embodiment of the present invention, the coating film drying time is 3-10 hours.
[0034] In one embodiment of the present invention, the coating film drying time is 5 hours.
[0035] In one embodiment of the present invention, the pre-expansion treatment in step (2) is specifically: the graphene oxide film is placed in a 1-3 mol / L ammonium bicarbonate solution and immersed in vacuum at room temperature for 10-40 minutes, followed by drying at 50-70°C for 1-3 hours, and then drying at 90-110°C for 15-45 minutes.
[0036] In one embodiment of the present invention, the dipping and drying steps are repeated twice.
[0037] In one embodiment of the present invention, the concentration of the ammonium bicarbonate solution is 2 mol / L.
[0038] In one embodiment of the present invention, the immersion time is 15 minutes.
[0039] In one embodiment of the present invention, the drying time at 60° C. is 2 hours.
[0040] In one embodiment of the present invention, the drying time at 100° C. is 30 minutes.
[0041] Since the coating thickness is at the centimeter level, if the dehydration rate is too fast during the drying and dehydration process, the graphene oxide film will crack and curl. The inventors found that by controlling the drying temperature and adjusting the appropriate drying steps, first drying at 50-70°C until most of the water evaporates, and then further drying at 90-110°C, the graphene oxide film can be prevented from cracking and curling.
[0042] In one embodiment of the present invention, the foaming treatment in step (3) is specifically: immersing the pre-expanded graphene oxide film in a 70-90% by mass hydrazine hydrate solution, foaming at 40-60° C. in vacuum for 2-4 hours, and then drying at 120° C. for 90-180 minutes.
[0043] In one embodiment of the present invention, the mass percentage of the hydrazine hydrate solution is 80%.
[0044] In one embodiment of the present invention, the foaming temperature is 50°C.
[0045] In one embodiment of the present invention, the foaming time is 3 hours.
[0046] In one embodiment of the present invention, the drying time is 120 minutes.
[0047] In one embodiment of the present invention, the temperature of the carbonization treatment in step (4) is 900-1400°C.
[0048] In one embodiment of the present invention, the temperature of the carbonization treatment is 1250°C.
[0049] In one embodiment of the present invention, the temperature of the graphitization treatment is 2600-3000°C.
[0050] In one embodiment of the present invention, the temperature of the graphitization treatment is 2800°C.
[0051] In one embodiment of the present invention, the carbonization treatment is performed under the protection of an inert gas.
[0052] In one embodiment of the present invention, the graphitization treatment is performed under the protection of an inert gas.
[0053] In one embodiment of the present invention, the inert gas is at least one selected from nitrogen, helium and argon.
[0054] In one embodiment of the present invention, the fluorination treatment in step (5) is gas phase fluorination, and intermittent vacuum treatment is performed during the gas phase fluorination process.
[0055] In one embodiment of the present invention, the specific process of the gas phase fluorination is as follows:
[0056] a. placing the carbonized and graphitized film in a closed fluorination reaction device;
[0057] b. Vacuum to below 10Pa;
[0058] c. Stop vacuuming and introduce gaseous fluorinating agent and inert gas;
[0059] d. After the pressure in the fluorination reaction device rises to normal pressure, continue to introduce the gaseous fluorinating agent and the inert gas and maintain for 2-10 minutes;
[0060] e. Repeat the above steps bd 10-100 times.
[0061] In one embodiment of the present invention, the flow ratio of the gaseous fluorinating agent to the inert gas is 1:1-10.
[0062] In one embodiment of the present invention, the flow rate of the gaseous fluorinating agent is 100-500 sccm, and the flow rate of the inert gas is 500-1000 sccm;
[0063] In one embodiment of the present invention, the gaseous fluorinating agent is F2 and / or XeF2.
[0064] In one embodiment of the present invention, the inert gas is at least one selected from nitrogen, helium and argon.
[0065] In one embodiment of the present invention, the gas phase fluorination is carried out at 180-220°C.
[0066] In one embodiment of the present invention, the gas phase fluorination is carried out at 200°C.
[0067] In one embodiment of the present invention, the surface of the reaction chamber of the fluorination reaction device is made of polytetrafluoroethylene or metal nickel.
[0068] In one embodiment of the present invention, the fluorination reaction device further comprises a tail gas absorption device, and the tail gas absorption device absorbs the tail gas of the fluorination reaction by using an alkaline solution.
[0069] In one embodiment of the present invention, the alkali solution is selected from at least one of potassium hydroxide, sodium hydroxide and calcium hydroxide.
[0070] In one embodiment of the present invention, the thickness of the fluorinated graphene insulating and thermally conductive film can be controlled by adjusting the pressure of a press.
[0071] Compared with the prior art, the technical effects achieved by the present invention are as follows:
[0072] (1) The fluorinated graphene insulating thermally conductive film of the present invention does not contain adhesives or second phase matrix, and can significantly reduce the thermal resistance of the film interface. The thermal conductivity and volume resistivity of the fluorinated graphene insulating thermally conductive film are in the following ranges: thermal conductivity is 550-800 W·(m·k) -1 (including 550W·(m·k) -1 ), and the volume resistivity is 1-10×10 13 Ω·cm; or thermal conductivity is 400-550W·(m·k) -1 (Excluding 550W·(m·k) -1 ), and the volume resistivity is greater than 10 14 Ω·cm;
[0073] (2) By pre-expanding and foaming the graphene oxide membrane, a rich porous network is constructed, which shortens the diffusion distance of the gaseous fluorinating agent during the fluorination process, making it easier for the gaseous fluorinating agent to react with the graphene oxide membrane, thereby improving the fluorination efficiency and achieving highly uniform fluorination;
[0074] (3) An innovative "breathing" gas-phase fluorination process was constructed, in which intermittent vacuum treatment was performed during the fluorination process. The fluorination process was cycled in a mode of vacuumization-ventilation and pressure increase-normal pressure maintenance, which can further enhance the penetration of the gaseous fluorinating agent into the graphene oxide film and further ensure the highly uniform fluorination of the graphene oxide film;
[0075] (4) The present invention not only provides a method for optimizing the preparation of fluorinated graphene insulating thermal conductive film in theory, but also can realize industrial-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 is a cross-sectional scanning electron microscope image of a graphene oxide film prepared according to one embodiment of the present invention;
[0077] Figure 2 is a cross-sectional scanning electron microscope image of a graphene oxide membrane having a porous network after foaming treatment according to one embodiment of the present invention;
[0078] Figure 3 3 is a scanning electron microscope image of the fluorinated graphene insulating thermally conductive film prepared according to Example 1 of the present invention. DETAILED DESCRIPTION
[0079] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0080] The technical solution of the present invention is described below by specific embodiments. It should be understood that one or more steps mentioned in the present invention do not exclude the existence of other methods and steps before and after the combination step, or other methods and steps can be inserted between these explicitly mentioned steps. It should also be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Unless otherwise specified, the numbering of each method step is only for the purpose of identifying each method step, and does not limit the order of arrangement of each method or limit the scope of implementation of the present invention. The change or adjustment of the relative relationship thereof can also be regarded as the scope of implementation of the present invention without substantial changes in the technical content.
[0081] The sources of the raw materials and instruments used in the examples are not particularly limited and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0082] Example 1
[0083] A method for preparing a fluorinated graphene insulating thermally conductive film comprises the following steps:
[0084] (1) Preparation of graphene oxide film: Weigh one part of 200 mesh flake graphite, 6 parts of potassium permanganate and 35 parts of concentrated sulfuric acid, prepare graphene oxide by Hummers method and prepare into slurry with a solid content of 4%, apply the slurry on a fiber filter cloth with a thickness of 1.2 cm, and then dry at 90° C. for 5 hours to obtain a graphene oxide film;
[0085] (2) Pre-expansion treatment: The dried film was immersed in a 2 mol / L ammonium bicarbonate solution at room temperature under vacuum for 15 minutes, then dried at 60°C for 2 hours, and the immersion and drying process was repeated twice, followed by drying at 100°C for 30 minutes;
[0086] (3) Foaming treatment: the pre-expanded film is immersed in 80% hydrazine hydrate solution, foamed at 50°C for 3 hours in vacuum, and then dried at 120°C for 120 minutes for later use;
[0087] (4) Carbonization and graphitization: The foamed and dried film is carbonized at 1250°C and graphitized at 2800°C under inert gas protection;
[0088] (5) Fluorination treatment: Place the graphitized film in a fluorination reaction chamber, then close the chamber and evacuate it. After evacuating to vacuum, introduce 150 sccm of F2 and 500 sccm of N2. After returning to normal pressure, continue to introduce the above-mentioned gases until the temperature reaches 200°C. Then turn off the gas, evacuate to 10 Pa, and then introduce the above-mentioned gases again to restore normal pressure and maintain for 5 minutes. Repeat the above-mentioned process of evacuating - ventilating and pressurizing - maintaining normal pressure for 5 minutes 20 times.
[0089] (6) The fluorinated graphene film is rolled to form a fluorinated graphene insulating thermally conductive film, and the thickness of the fluorinated graphene insulating thermally conductive film can be controlled by adjusting the pressure of a press.
[0090] The graphene oxide film obtained by step (1) in Example 1, the graphene oxide film after foaming treatment obtained by step (3), and the final fluorinated graphene insulating thermal conductive film product were characterized by SEM (scanning electron microscope) to obtain Figure 1 , Figure 2 and Figure 3 .
[0091] from Figure 1 , Figure 2 By comparison, it can be seen that Figure 1 The cross section of the graphene oxide film is relatively dense overall, with only a small amount of pores in some areas. Figure 2The graphene oxide membrane has been pre-expanded and foamed, and the entire cross-section is full of pores, indicating that a rich porous network has been constructed in the graphene oxide membrane through pre-expanding and foaming treatments. This structure is conducive to the absorption and penetration of the fluorinating agent in the later fluorination process, thereby improving the degree and uniformity of fluorination.
[0092] from Figure 3 It can be seen that the fluorinated graphene insulating thermal conductive film product obtained by calendering is very compact, with almost no gaps between layers. This is because after fluorination, the interplanar spacing of fluorinated graphene increases, its in-plane rigidity is significantly improved, its self-lubricating ability is enhanced, and the introduction of fluorine atoms reduces the surface energy. All these factors make it easy for fluorinated graphene to be calendered to the required thickness without the phenomenon of rebound after compression.
[0093] At the same time, it was characterized by a thermal conductivity test device and a volume resistance test device. The in-plane thermal conductivity of the fluorinated graphene insulating thermal conductive film prepared by the method of Example 1 was 800 W·(m·k) -1 , the volume resistivity is 2.1×10 13 Ω·cm. Through the data analysis during the experiment, it can also be found that the insulation performance and thermal conductivity of fluorinated graphene are highly correlated with the degree of fluorination. The higher the degree of fluorination, the stronger the insulation performance and the smaller the thermal conductivity. This is because the intervention of fluorine atoms covalently combines with the carbon atoms of graphene to form insulating CF covalent bonds, which leads to enhanced insulation performance. When F / C is greater than 1, graphene directly becomes an insulator, but at the same time, graphene oxide will also change from sp2 hybrid structure to sp3 hybrid structure as the fluorination reaction proceeds, resulting in a decrease in the thermal conductivity of fluorinated graphene. The F / C ratio can be judged by XPS characterization and resistivity volume ratio.
[0094] Example 2
[0095] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that: in step (2), the pre-expansion treatment immersion time is 40 minutes, the 60°C drying time is 3 hours, the 100°C drying time is 45 minutes, and the immersion and drying processes are not repeated; in step (3), the foaming treatment time is 4 hours, and the drying time is 150 minutes.
[0096] Example 3
[0097] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that: in step (2), the pre-expansion treatment immersion time is 20 minutes, the 60°C drying time is 1 hour, and the 100°C drying time is 15 minutes; in step (3), the foaming treatment time is 2 hours and the drying time is 180 minutes.
[0098] Example 4
[0099] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that: step (5) introduces 200 sccm of F2 and 500 sccm of N2, and repeats the vacuuming-ventilation-pressurization-normal pressure maintenance process 25 times.
[0100] Example 5
[0101] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that: step (5) introducing 400 sccm of F2 and 800 sccm of N2, and repeating the vacuuming-ventilation-pressurization-normal pressure maintenance process 30 times.
[0102] Example 6
[0103] A method for preparing a fluorinated graphene insulating thermally conductive film, which differs from Example 1 in that: step (5) introducing 400 sccm of F2 and 500 sccm of N2, and repeating the process of vacuuming-ventilating and pressurizing-maintaining at normal pressure 40 times.
[0104] Example 7
[0105] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that: step (5) introducing 500 sccm of F2 and 1000 sccm of N2, and repeating the vacuuming-ventilation-pressurization-normal pressure maintenance process 25 times.
[0106] Example 8
[0107] A method for preparing a fluorinated graphene insulating thermally conductive film, which differs from Example 1 in that: step (5) introducing 500 sccm of F2 and 500 sccm of N2, and repeating the process of vacuuming-ventilating and pressurizing-maintaining at normal pressure 40 times.
[0108] Example 9
[0109] A method for preparing a fluorinated graphene insulating thermally conductive film, which differs from Example 1 in that: step (5) introducing 500 sccm of XeF2 and 500 sccm of N2, and repeating the process of vacuuming-ventilating and pressurizing-maintaining at normal pressure 40 times.
[0110] Comparative Example 1
[0111] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that the pre-expansion treatment step (2) is not performed.
[0112] Comparative Example 2
[0113] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that the foaming treatment step (3) is not performed.
[0114] Comparative Example 3
[0115] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that the carbonization treatment and graphitization treatment steps of step (4) are not performed.
[0116] Comparative Example 4
[0117] A method for preparing a fluorinated graphene insulating thermally conductive film, which is different from Example 1 in that the fluorination step in step (5) is not subjected to intermittent vacuum treatment.
[0118] The samples prepared in Examples 1-8 and Comparative Examples 1-4 were subjected to thermal conductivity tests and volume resistance tests, and the test results were shown in Table 1 below:
[0119] Table 1: Thermal conductivity test and volume resistance test results
[0120] Test samples <![CDATA[In-plane thermal conductivity (W·(m·k) -1 )]]> Volume resistivity (Ω·cm) Example 1 800 <![CDATA[2.1×10 13 <!-- 6 -->]]> Example 2 694 <![CDATA[1.6×10 13 ]]> Example 3 576 <![CDATA[1.0×10 13 ]]> Example 4 625 <![CDATA[9.0×10 13 ]]> Example 5 515 <![CDATA[5.2×10 14 ]]> Example 6 540 <![CDATA[2.3×10 14 ]]> Example 7 509 <![CDATA[6.1×10 14 ]]> Example 8 400 <![CDATA[1.9×10 15 ]]> Example 9 465 <![CDATA[5.1×10 14 ]]> Comparative Example 1 506 <![CDATA[4.6×10 12 ]]> Comparative Example 2 425 <![CDATA[7×10 11 ]]> Comparative Example 3 321 <![CDATA[6.5×10 13 ]]> Comparative Example 4 714 <![CDATA[1.5×10 12 ]]>
[0121] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A method for preparing a fluorinated graphene insulating thermally conductive film, characterized in that: The preparation method comprises the following steps: (1) Preparation of graphene oxide film; (2) pre-expanding the graphene oxide film; (3) performing foaming treatment on the film that has undergone the pre-expansion treatment; (4) subjecting the foamed film to carbonization and graphitization; (5) performing a fluorination treatment on the film that has undergone the carbonization treatment and the graphitization treatment to obtain a fluorinated graphene film; (6) rolling the fluorinated graphene film to form the fluorinated graphene insulating and thermally conductive film; The pre-expansion treatment in step (2) is specifically as follows: the graphene oxide film is immersed in a 1-3 mol / L ammonium bicarbonate solution under vacuum at room temperature for 10-40 minutes, followed by drying at 50-70°C for 1-3 hours, and then drying at 90-110°C for 15-45 minutes; The foaming treatment in step (3) is specifically as follows: immersing the pre-expanded graphene oxide film in a 70-90% by mass hydrazine hydrate solution, foaming at 40-60° C. in vacuum for 2-4 hours, and then drying at 120° C. for 90-180 minutes; The fluorination treatment in step (5) is gas phase fluorination, and intermittent vacuum treatment is performed during the gas phase fluorination process; The specific process of the gas phase fluorination is as follows: a. placing the carbonized and graphitized film in a closed fluorination reaction device; b. Vacuum to below 10Pa; c. Stop vacuuming and introduce gaseous fluorinating agent and inert gas; d. After the pressure in the fluorination reaction device rises to normal pressure, continue to introduce the gaseous fluorinating agent and the inert gas and maintain for 2-10 minutes; e. Repeat the above steps bd 10-100 times.
2. The preparation method according to claim 1, characterized in that: The graphene oxide film in step (1) is obtained by preparing graphene oxide slurry by Hummers method, and then coating and drying the slurry.
3. The preparation method according to claim 2, characterized in that: The coating film has a thickness of 1-1.5 cm.
4. The preparation method according to claim 2, characterized in that: The thickness of the coating film is 1.1-1.3 cm.
5. The preparation method according to claim 2, characterized in that: The thickness of the coating film is 1.2 cm.
6. The preparation method according to claim 1, characterized in that: The impregnation and drying steps are repeated twice; and / or, the concentration of the ammonium bicarbonate solution is 2 mol / L; and / or, the impregnation time is 15 minutes; and / or, the drying temperature at 50-70°C is 60°C, and the drying time is 2 hours; and / or, the drying temperature at 90-110°C is 100°C, and the drying time is 30 minutes.
7. The preparation method according to claim 1, characterized in that: The mass percentage concentration of the hydrazine hydrate solution is 80%; and / or the foaming temperature is 50° C.; and / or the foaming time is 3 hours; and / or the drying time is 120 minutes.
8. The preparation method according to claim 1, characterized in that: The temperature of the carbonization treatment in step (4) is 900-1400°C; And / or, the temperature of the graphitization treatment is 2600-3000°C; And / or, the carbonization treatment is carried out under the protection of an inert gas; And / or, the graphitization treatment is performed under the protection of an inert gas.
9. The preparation method according to claim 8, characterized in that: The temperature of the carbonization treatment is 1250°C; And / or, the temperature of the graphitization treatment is 2800°C.
10. The preparation method according to claim 1, characterized in that: The flow ratio of the gaseous fluorinating agent to the inert gas is 1:1-10; and / or, the gaseous fluorinating agent is F2 and / or XeF2; And / or, the inert gas is at least one selected from nitrogen, helium and argon.
11. The preparation method according to claim 10, characterized in that: The flow rate of the gaseous fluorinating agent is 100-500 sccm, and the flow rate of the inert gas is 500-1000 sccm.
12. The preparation method according to claim 1, characterized in that: The gas phase fluorination is carried out at 180-220°C.
13. The preparation method according to claim 1, characterized in that: The gas phase fluorination was carried out at 200°C.
14. A fluorinated graphene insulating thermally conductive film, characterized in that: According to the preparation method according to any one of claims 1 to 13, the fluorinated graphene insulating thermally conductive film has no second phase matrix added, and the thermal conductivity and volume resistivity of the fluorinated graphene insulating thermally conductive film are in the following numerical ranges: Thermal conductivity is 550-800W∙(m∙K) -1 (including 550W∙(m∙k) -1 ), and the volume resistivity is 1-10×10 13 Ω∙cm; Or thermal conductivity is 400-550W∙(m∙K) -1 (Excluding 550W∙(m∙k) -1 ), and the volume resistivity is greater than 10 14 Ω∙cm.