Method for testing and quantifying group iii indium and group v arsenic oxides in indium arsenide
By combining wet etching with citric acid and hydrochloric acid with microscopy and X-ray analysis, the problem of cumbersome operation in indium arsenide testing methods has been solved, enabling rapid detection and quantification of Group III indium and Group V arsenic oxides.
Patent Information
- Application Number
- CN202310483934.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing methods for testing indium arsenide are cumbersome and make it difficult to efficiently detect and quantify the presence of Group III indium and Group V arsenic oxides.
Indium arsenide substrates were etched twice using a wet etching method with citric acid and hydrochloric acid. The presence and proportion of group III indium and group V arsenide oxides were determined and quantified by combining polarized light microscopy, scanning electron microscopy and X-ray energy dispersive analysis.
The detection process is simplified, enabling rapid and convenient identification and quantification of the oxide composition on the surface of indium arsenide, thus improving detection efficiency and accuracy.
Smart Images

Figure CN116380959B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of semiconductor materials technology, specifically to a method for testing and quantifying group III indium and group V arsenic oxides in indium arsenide. Background Technology
[0002] Indium arsenide is hailed as a fourth-generation semiconductor material, possessing a narrow bandgap (Eg = 0.356 eV) and high electron mobility (33000 cm⁻¹). 2 / V·sec), high intrinsic carrier concentration (1.25×10⁻⁶). 15 / cm 3 It possesses excellent properties such as , and its lattice constant is . The lattice constant of gallium antimonide Because of their very close similarity, lattice-matched epitaxial materials such as GaSb, GaInSb, InAsSb, GaAsSb, InAsPSb, and AlGaSb can be grown on indium arsenide, which can be used to fabricate lasers, infrared detectors, etc. Type II superlattices, represented by InAs / GaSb and InAs / GaInSb, are multilayer film materials formed by alternating thin layers of two different components in nanoscale form. These materials exhibit high product uniformity, high yield, high operating temperature, and advantages such as adjustable bandgap and wide spectral coverage, resulting in infrared detectors with high detection efficiency.
[0003] These performance characteristics of infrared detectors are achieved based on high-quality epitaxial materials. Defects in the epitaxial layer mainly originate from two sources. First, defects are generated during the epitaxial process, known as process-induced defects. Second, some defects originate from the substrate (including the substrate single crystal material and the substrate surface), known as extension defects. An important parameter on the substrate surface is the native oxide layer, which is generated by the combined effects of chemical mechanical polishing and subsequent wet chemical cleaning. Since indium arsenide is a zincblende crystal, its lattice is composed of a face-centered cubic lattice formed by group III In atoms and group V As atoms, which are displaced along the body diagonal. In readily reacts with acidic solutions, while group V atoms readily react with alkaline solutions. The main oxidation states of indium are +1 and +3, and the main oxide forms are In₂O and In₂O₃. In₂O is easily desorbed at high temperatures, while In₂O₃ is very stable at high temperatures and does not easily desorb. The less desorbable In₂O₃ readily serves as a nucleation source for preferential growth. Therefore, preparing a substrate interface with active controllability and easy desorption to eliminate or suppress epitaxial defects at their source is crucial. Therefore, it is particularly important to detect whether the InAs substrate has an easily desorbable interface after cleaning.
[0004] Traditional detection methods use XPS (Extreme Photolysis), which works by irradiating the sample with X-rays, exciting inner-shell or valence electrons in atoms or molecules to be emitted. These emitted electrons are called photoelectrons. The energy of the photoelectrons can be measured, and a photoelectron energy spectrum can be created by plotting the kinetic energy / binding energy (Eb = hv light energy - Ek kinetic energy - w work function) on the x-axis and the relative intensity (pulse / s) on the y-axis. This provides information about the sample. The sample size is generally less than 5*5*3cm, with both sides clearly marked, and the sample must be dry and have a smooth surface. Traditional methods use wet chemical etching and require a dedicated XPS testing facility, specifying the required sample, making the entire testing process cumbersome. Summary of the Invention
[0005] (a) Technical problems to be solved
[0006] To address the aforementioned issues, this disclosure provides a method for detecting and quantifying group III indium and group V arsenic oxides in indium arsenide, which at least partially solves the technical problems of cumbersome operation in the detection methods for group III indium and group V arsenic oxides in indium arsenide.
[0007] (II) Technical Solution
[0008] This disclosure provides a method for testing group III indium and group V arsenic oxides in indium arsenide, comprising: S1, placing an indium arsenide substrate in a citric acid solution for a first etching, and then rinsing with deionized water; wherein a native oxide layer is formed on the surface of the indium arsenide substrate; S2, placing the indium arsenide substrate obtained in S1 in a hydrochloric acid solution for a second etching, and then rinsing with deionized water and drying; S3, using a polarizing microscope to examine and observe the indium arsenide substrate obtained in S2 under a dark field to determine whether particles are present on the surface of the indium arsenide substrate; S4, if particles are present on the surface of the indium arsenide substrate, the elemental percentage of group III indium in the native oxide layer is higher than the elemental percentage of group V arsenic; otherwise, the elemental percentage of group V arsenic in the native oxide layer is not lower than the elemental percentage of group III indium.
[0009] Furthermore, the citric acid solution in S1 comprises a mixed solution consisting of citric acid monohydrate, hydrogen peroxide, and deionized water.
[0010] Furthermore, the ratio of citric acid monohydrate, hydrogen peroxide, and deionized water is [10-50]g: [10-50]ml: [500-1300]ml.
[0011] Furthermore, the corrosion time range for the first corrosion in S1 is 20–100 seconds, and the corrosion temperature is room temperature.
[0012] Furthermore, the hydrochloric acid solution in S2 comprises a mixed solution consisting of hydrochloric acid with a mass concentration of 30% and deionized water.
[0013] Furthermore, the ratio of 30% hydrochloric acid to deionized water is [10-50] ml: [500-1300] ml.
[0014] Furthermore, the corrosion time range for the second corrosion in S2 is 20–100 seconds, and the corrosion temperature is room temperature.
[0015] Furthermore, the size range of particles observed by polarized light microscopy in S3 is in the hundreds of nanometers.
[0016] Another aspect of this disclosure provides a quantitative method for indium III and arsenic V oxides in indium arsenide, comprising: S1, placing an indium arsenide substrate in a citric acid solution for a first etching, followed by rinsing with deionized water; wherein a native oxide layer is formed on the surface of the indium arsenide substrate; S2, placing the indium arsenide substrate obtained in S1 in a hydrochloric acid solution for a second etching, followed by rinsing with deionized water and drying; S3, using a polarizing microscope to examine and observe the indium arsenide substrate obtained in S2 under a dark field to determine whether particles are present on the surface of the indium arsenide substrate; S4, in response to the presence of particles on the surface of the indium arsenide substrate, observing the morphology of the particles using a scanning electron microscope; S5, using X-ray energy dispersive analysis to perform elemental analysis on the particles to obtain the elemental percentages of group III indium, group V arsenic, and oxygen.
[0017] Furthermore, it also includes: S6, which calculates the composition of the natural oxide layer based on the element percentages.
[0018] (III) Beneficial Effects
[0019] The method and quantification method for detecting and quantifying Group III indium and Group V arsenic oxides in indium arsenide disclosed herein involve first etching the indium arsenide substrate with citric acid solution to react with the native oxide layer on the surface of the indium arsenide substrate and remove some of the oxides in the native oxide layer; then, a second etching method is performed on the indium arsenide substrate with hydrochloric acid solution to further react with the oxides, remove the Group III indium components, and promote the formation of InAs. x O y Finally, the presence of InAs on the surface was observed using a polarizing microscope. x O y The particles allow us to determine the atomic percentages of Group III indium and Group V arsenic in the native oxide layer. Furthermore, scanning electron microscopy and X-ray energy dispersive spectroscopy can be used for quantitative analysis of Group III indium and Group V arsenic oxides. Attached Figure Description
[0020] Figure 1A flowchart illustrating a method for testing group III indium and group V arsenic oxides in indium arsenide according to embodiments of this disclosure is shown schematically.
[0021] Figure 2 A schematic diagram illustrating the In, As, and O ternary equilibrium phase diagram according to an embodiment of this disclosure is shown.
[0022] Figure 3 The illustration schematically shows a dark-field microscopic image of an indium arsenide sample after etching with an etching solution according to an embodiment of the present disclosure;
[0023] Figure 4 A flowchart illustrating a method for quantifying group III indium and group V arsenic oxides in indium arsenide according to embodiments of the present disclosure is shown schematically.
[0024] Figure 5 The illustration shows images of the morphology and top cross-section of an indium arsenide sample after etching with an etching solution, as observed by scanning electron microscopy according to an embodiment of the present disclosure. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of this disclosure clearer, the following detailed description is provided in conjunction with specific embodiments and the accompanying drawings.
[0026] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit this disclosure. The terms “comprising,” “including,” etc., as used herein indicate the presence of the stated features, steps, operations, and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, or components.
[0027] Traditional methods for testing group III and group V arsenic oxides in indium arsenide steel employ X-ray photoelectron spectroscopy (XPS), a cumbersome process. Therefore, this disclosure provides a method for testing and quantifying group III and group V arsenic oxides in indium arsenide using wet etching, which can be easily and conveniently performed using conventional microscopy techniques.
[0028] This disclosure provides a method for testing group III indium and group V arsenic oxides in indium arsenide. Please refer to [link to relevant documentation]. Figure 1The process includes: S1, etching the indium arsenide substrate in citric acid solution for the first time, followed by rinsing with deionized water; wherein a native oxide layer is formed on the surface of the indium arsenide substrate; S2, etching the indium arsenide substrate obtained in S1 in hydrochloric acid solution for the second time, followed by rinsing with deionized water and drying; S3, examining the indium arsenide substrate obtained in S2 under a dark field using a polarizing microscope to determine whether particles are present on the surface of the indium arsenide substrate; S4, if particles are present on the surface of the indium arsenide substrate, the percentage of Group III indium in the native oxide layer is higher than the percentage of Group V arsenic; otherwise, the percentage of Group V arsenic in the native oxide layer is not lower than the percentage of Group III indium.
[0029] This disclosure employs wet etching technology for inspection, utilizing the In, As, and O ternary phase diagram as a reference based on the principles of wet etching (e.g., ...). Figure 2 (As shown) The interface between group III indium and group V arsenic can be prepared by adjusting the changes in the etchant, which facilitates desorption.
[0030] This method involves first etching an indium arsenide substrate with citric acid solution, which reacts with the native oxide layer on the substrate surface to remove some of the oxides. Then, a second etching process is performed with hydrochloric acid solution to further react with the oxides, removing Group III indium and promoting the formation of InAsxOy. Finally, a polarizing microscope is used to observe the presence of InAsxOy particles on the surface, thereby determining the atomic percentages of Group III indium and Group V arsenic in the native oxide layer.
[0031] Based on the above embodiments, the citric acid solution in S1 includes a mixed solution composed of citric acid monohydrate, hydrogen peroxide, and deionized water. The ratio of citric acid monohydrate, hydrogen peroxide, and deionized water is in the range of [10–50] g : [10–50] ml : [500–1300] ml.
[0032] Citric acid is mainly used to react with oxides in the oxide layer on the surface of indium arsenide substrates, effectively removing surface oxides, especially group III oxides. The reaction formula is as follows:
[0033] Reaction 1: In₂O₃ + C₆H₈O₇ → [In(C₂H₄O₆)(H₂O)] + H₂O + 2H₂O +
[0034] Hydrogen peroxide is mainly used to promote the formation of oxides, and the reaction formula is as follows:
[0035] Reaction 2: 2InAs + H2O2 → In2O3 + As2O5 + 6H2O.
[0036] The ratio of citric acid monohydrate, hydrogen peroxide, and deionized water within the above range is beneficial for: ① the action of hydrogen peroxide to facilitate the removal of Group III oxides and Group V oxides according to reaction formula 2; ② the action of citric acid to facilitate the removal of some Group III oxides according to reaction formula 1.
[0037] Based on the above embodiments, the hydrochloric acid solution in S2 comprises a mixed solution of hydrochloric acid with a mass concentration of 30% and deionized water. The ratio of the 30% hydrochloric acid to the deionized water is in the range of [10–50] ml : [500–1300] ml.
[0038] Hydrochloric acid has the following three functions:
[0039] (1) Corrosion of indium arsenide oxides, especially indium oxides, by the following reaction:
[0040] Reaction 3: In₂O₃ + 2HCl → InCl₃ + H₂O
[0041] (2) It is an anisotropic corrosive acid that reacts with the indium arsenide substrate, and the reaction formula is as follows:
[0042] Reaction 4: InAs + 2HCl → InCl3 + AsH3 (gas)
[0043] (3) And the following reaction is easily carried out in the hydrochloric acid environment:
[0044] Reaction 5: In₂O₃ + As₂O₅ → InAs x O y .
[0045] Diluting hydrochloric acid with deionized water facilitates the removal of some group III oxides and prevents the formation of some group III oxides according to reactions 3 and 4 above, regulates the ratio of group III oxides to group V oxides, and promotes the formation of reaction 5.
[0046] It should be noted that the order of the two etching processes cannot be substituted, as this is determined based on the reaction mechanism. Hydrogen peroxide rapidly promotes oxide formation, while citric acid only reacts with the indium arsenide substrate oxide, removing some of the oxide. Hydrochloric acid can further react with the oxide and also react with the substrate, removing In. In this acidic environment, the following reactions are easily facilitated:
[0047] In₂O₃ + As₂O₅ → InAs x O y
[0048] This directs the reaction toward arsenic-rich oxides.
[0049] After a second etching with hydrochloric acid, the sample was rinsed with deionized water and dried with nitrogen.
[0050] Based on the above embodiments, the corrosion time range for the first corrosion in S1 is 20-100 seconds, and the corrosion temperature is room temperature. The corrosion time range for the second corrosion in S2 is 20-100 seconds, and the corrosion temperature is room temperature.
[0051] The two corrosion processes disclosed herein have short corrosion times and can be carried out at room temperature, making the conditions mild and the operation simple.
[0052] Based on the above embodiments, the size range of particles observed by the polarizing microscope in S3 is in the hundreds of nanometers.
[0053] The particles are basically InAs x O y A small amount of In₂O₃ may also be present. After the above etching process, the particle size ranges to the hundreds of nanometers. Dark-field observation under a polarizing microscope allows for easy acquisition of small and clear particles.
[0054] Polarizing microscopes have two advantages over ordinary microscopes: (1) single refractive index and birefringence; (2) polarization characteristics of light. These two advantages enable the microscope to observe surface particles in a dark field. Using well-prepared polished discs (sample A and sample B), the above-mentioned solution etching process was performed. After etching, the images were observed in a dark field using a microscope, as shown in the following figures. Figure 3 As shown, the image of sample A is as follows: Figure 3 As shown in (a), the image of sample B is as follows: Figure 3 As shown in (b), it can be seen that the surface of sample A has a relatively large number of particles (e.g., ...). Figure 3 As shown in the circled area in (a), sample B has fewer particles on its surface. Therefore, it can be determined that the percentage of indium in the natural oxide layer on the surface of sample A is higher.
[0055] Compared to group V oxides, which are readily soluble in water, indium oxides are not easily soluble in water, especially since In2O3 particles are stable. Therefore, indium oxides generally exist in granular form on the substrate surface.
[0056] This disclosure also provides a quantitative method for indium III and arsenic V oxides in indium arsenide, such as... Figure 4As shown, the process includes: S1, placing the indium arsenide substrate in a citric acid solution for the first etching, followed by rinsing with deionized water; wherein a natural oxide layer is formed on the surface of the indium arsenide substrate; S2, placing the indium arsenide substrate obtained in S1 in a hydrochloric acid solution for the second etching, followed by rinsing with deionized water and drying; S3, using a polarizing microscope to examine the indium arsenide substrate obtained in S2 under a dark field to determine whether particles are present on the surface of the indium arsenide substrate; S4, in response to the presence of particles on the surface of the indium arsenide substrate, observing the morphology of the particles using a scanning electron microscope (SEM); S5, using the energy dispersive analysis of X-rays (EDAX) method to perform elemental analysis on the particles, obtaining the elemental percentages of Group III indium, Group V arsenic, and oxygen.
[0057] Steps S1 to S3 of this quantitative method are the same as those of the above-described test method, and will not be repeated here. Furthermore, SEM can be used to observe the morphology of the particles, primarily to observe InAs. x O y The morphology of the crystals was determined; then elemental analysis was performed using EDAX.
[0058] SEM (Scanning Electron Microscopy) observation of morphology is used to determine the morphology and location of particles. Then, EDAX is used to calibrate the composition at that location; otherwise, the composition at the location where the particles were generated is not that of the particle.
[0059] According to the above embodiments, such as Figure 5 As shown in the figure, the morphology of the particles observed by SEM is as follows. Figure 5 As shown in (a), the top cross-section of the particle observed by SEM is as follows. Figure 5 As shown in (b).
[0060] Based on the above embodiments, the method further includes: S6, calculating the composition of the compound in the natural oxide layer according to the element percentage.
[0061] According to the above embodiments, the two samples (sample A and sample B) were calibrated using EDAX, and the calibration results are shown in Table 1.
[0062] Table 1
[0063]
[0064] The composition of the compounds disclosed herein is obtained through the conversion of elemental percentages. For example, in sample A, In accounts for 15.45%, As accounts for 53.73%, and O accounts for 30.82%, then the resulting compound is In. 15.45 As 53.7 3O 30.82Then, assuming there is 1 In atom, the number of other atoms is divided by 15.45 of the In atomic percentage, yielding approximately 3 As and 2 O atoms. This results in the composition InAs3O2. Further evidence shows that sample B contains a relatively high amount of Group V arsenic oxides.
[0065] Therefore, the method disclosed herein can detect Group III indium and Group V arsenic oxides in indium arsenide, and can further quantify Group III indium and Group V arsenic oxides.
[0066] The specific embodiments described above further illustrate the purpose, technical solutions, and beneficial effects of this disclosure. It should be understood that the above descriptions are merely specific embodiments of this disclosure and are not intended to limit this disclosure. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the protection scope of this disclosure.
Claims
1. A method for testing group III indium and group V arsenic oxides in indium arsenide, characterized in that, include: S1, the indium arsenide substrate is placed in a citric acid solution for the first etching, and then rinsed with deionized water; wherein, a natural oxide layer is formed on the surface of the indium arsenide substrate; the citric acid solution includes a mixed solution composed of citric acid monohydrate, hydrogen peroxide and deionized water; S2, the indium arsenide substrate obtained in S1 is placed in a hydrochloric acid solution for a second etching, then rinsed with deionized water and dried; the hydrochloric acid solution is a hydrochloric acid solution diluted with deionized water, so that the reaction is directed towards the arsenic-rich oxide. S3. Use a polarizing microscope to examine and observe the indium arsenide substrate obtained in S2 under a dark field to determine whether there are particles on the surface of the indium arsenide substrate. S4. If particles are present on the surface of the indium arsenide substrate, the elemental percentage of group III indium in the native oxide layer is higher than that of group V arsenic; otherwise, the elemental percentage of group V arsenic in the native oxide layer is not lower than that of group III indium.
2. The method for testing group III indium and group V arsenic oxides in indium arsenide according to claim 1, characterized in that, The ratio of citric acid monohydrate, hydrogen peroxide, and deionized water is [10~50]g: [10~50]ml: [500~1300]ml.
3. The method for testing group III indium and group V arsenic oxides in indium arsenide according to claim 1, characterized in that, The corrosion time range for the first corrosion in S1 is 20~100s, and the corrosion temperature is room temperature.
4. The method for testing group III indium and group V arsenic oxides in indium arsenide according to claim 1, characterized in that, The hydrochloric acid solution in S2 comprises a mixed solution consisting of hydrochloric acid with a mass concentration of 30% and deionized water.
5. The method for testing group III indium and group V arsenic oxides in indium arsenide according to claim 4, characterized in that, The ratio of 30% hydrochloric acid to deionized water is [10~50] ml: [500~1300] ml.
6. The method for testing group III indium and group V arsenic oxides in indium arsenide according to claim 1, characterized in that, The second corrosion in S2 has a corrosion time range of 20~100s and a corrosion temperature of room temperature.
7. The method for testing group III indium and group V arsenic oxides in indium arsenide according to claim 1, characterized in that, The size range of particles observed by the polarizing microscope in S3 is in the hundreds of nanometers.
8. A method for quantitatively analyzing Group III indium and Group V arsenic oxides in indium arsenide, characterized in that, include: S1, the indium arsenide substrate is placed in a citric acid solution for the first etching, and then rinsed with deionized water; wherein, a natural oxide layer is formed on the surface of the indium arsenide substrate; the citric acid solution includes a mixed solution composed of citric acid monohydrate, hydrogen peroxide and deionized water; S2, the indium arsenide substrate obtained in S1 is placed in a hydrochloric acid solution for a second etching, then rinsed with deionized water and dried; the hydrochloric acid solution is a hydrochloric acid solution diluted with deionized water, so that the reaction is directed towards the arsenic-rich oxide. S3. Use a polarizing microscope to examine and observe the indium arsenide substrate obtained in S2 under a dark field to determine whether there are particles on the surface of the indium arsenide substrate. S4, in response to the presence of particles on the surface of the indium arsenide substrate, the morphology of the particles is observed using a scanning electron microscope; S5. The particles are subjected to elemental analysis using X-ray energy dispersive analysis to obtain the elemental percentages of Group III indium, Group V arsenic, and oxygen.
9. The method for quantitatively analyzing Group III indium and Group V arsenic oxides in indium arsenide according to claim 8, characterized in that, Also includes: S6, the composition of the compound in the natural oxide layer is calculated based on the element percentages.
Citation Information
Patent Citations
Method for controlling III-group indium oxide and V-group arsenic oxide in indium arsenide
CN115522263A