A low-temperature green preparation method of titanium phosphate salt and composite material with NASICON structure

By using metatitanic acid and phosphoric acid as raw materials, combined with wet micro-heat stirring and low-temperature sintering technology, the problems of high raw materials and harmful gas emissions in the preparation of NASICON structural titanium phosphate materials are solved, and low-temperature with abundant resources and low prices are achieved Preparation, high purity and good crystallinity products were obtained.

CN116395655BActive Publication Date: 2024-11-15JIANGSU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310197686.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-11-15
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

In the existing preparation method of NASICON structural titanium phosphate salt material, the raw material cost is high, the sintering temperature is high, and harmful gases are generated, making it difficult to achieve low-temperature green preparation.

Method used

Using metatitanic acid and phosphoric acid as raw materials, titanium phosphate salt and composite materials are prepared by wet micro-heat stirring, solid-liquid separation and low-temperature sintering. An alkali metal source, carbon source and acid catalyst are used to reduce the preparation temperature to 350-450. ℃ to avoid harmful gas emissions.

Benefits of technology

The large-scale preparation of NASICON structural titanium phosphate materials with rich resources and low prices has been achieved, which reduces energy consumption, avoids harmful gas emissions, and produces high-purity and good crystallinity products at lower temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116395655B_ABST
    Figure CN116395655B_ABST
Patent Text Reader

Abstract

The invention discloses a low-temperature green preparation method of a titanium phosphate salt and a composite material with a NASICON structure, wherein an alkali metal source, a titanium source, a phosphorus source, a carbon source, water, and an acidic catalyst are put into a reactor together; the reaction mixture is stirred under heating conditions, the heating temperature is 80-100°C, and the time is 2-10 hours; the solid-liquid separation of the reacted mixture is carried out, and the reaction mixture is dried to obtain a powdery precursor for preparing a corresponding polyphosphate and a composite material; the precursor is calcined in an inert or air atmosphere, and the titanium phosphate salt and the composite material are obtained after natural cooling. In this scheme, not only is the raw material source abundant and the price low, but also there are few by-products and no harmful gas discharge, which is environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inorganic material preparation, and in particular to a low-temperature green preparation method of polyphosphate and composite materials. Background Art

[0002] In the process of transformation from old to new energy forms, utilization and development of new energy, secondary batteries play an important role. Although lead-acid batteries and lithium-ion batteries are currently widely used in mobile power supplies, energy storage and other fields, new battery systems are beginning to develop rapidly due to their respective defects, and emerging aqueous batteries have attracted much attention. Titanium phosphates with NASICON structure (LiTi2(PO4)3, NaTi2(PO4)3NaTi2, KTi2(PO4)3) are polyanionic materials. The three-dimensional polyanionic skeleton gives them the advantages of high ion conductivity and high structural stability. As an alkali metal ion battery electrode material, it can remain stable during the charge and discharge process, and the volume change is almost zero.

[0003] At present, the most common method for preparing such materials is high-temperature solid-phase synthesis, that is, the required raw materials are mixed evenly and then sintered at high temperature. Generally, high temperature and time are required. The temperature of the heat treatment of the currently disclosed technology is almost 750 ° C, and the time required is also very long, generally ranging from 2 to 20 hours. For example, patent CN115275152 discloses a method for preparing lithium titanium phosphate, with a treatment temperature of 750 ° C and a time of 5 hours; patent CN 113764620 discloses a method for preparing sodium titanium phosphate, with a treatment temperature of 750 ° C and a time of 8 hours; patent CN113394382 discloses a method for preparing potassium titanium phosphate, with a treatment temperature of 750 ° C. The use of long-term high-temperature treatment not only puts higher requirements on the equipment, but also has high energy consumption, which is not in line with the dual-carbon development direction. In addition, in terms of titanium source selection, tetrabutyl titanate is often used to obtain high-performance materials; ammonium dihydrogen phosphate is often used as the phosphorus source. At present, there are few technologies that use cheap metatitanic acid and phosphoric acid as raw materials. Phosphoric acid is highly acidic and is a viscous liquid. It is difficult to process it with other raw materials into a highly workable powder precursor. Therefore, there are still many technical difficulties in the large-scale preparation of sodium titanium phosphate using phosphoric acid as a raw material.

[0004] Therefore, it is of application value to develop a method for preparing titanium phosphate with NASICON structure at low temperature using inexpensive titanic acid and phosphoric acid as raw materials. Summary of the invention

[0005] The purpose of the present invention is to address the problems of high raw material cost, high sintering temperature, and generation of tail gas such as ammonia in the existing preparation technology of titanium phosphate with NASICON structure, and to propose a new preparation method of titanium phosphate with NASICON structure and composite material. The preparation method of the present invention can greatly reduce the preparation cost, does not generate harmful gases, and is environmentally friendly.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a titanium phosphate salt and a composite material with a NASICON structure. The method comprises: using metatitanic acid as a titanium source; using phosphoric acid or dilithium (sodium, potassium) phosphate as a phosphorus source; using dilithium (sodium, potassium) phosphate, lithium (sodium, potassium) citrate, lithium oxalate, lithium tartrate, and lithium malate as alkali metal sources; using lithium citrate, lithium oxalate, lithium tartrate, lithium malate, glucose, sucrose, carbon nanotubes, and graphene as carbon sources, and then subjecting the titanium phosphate salt or the titanium phosphate composite material to wet-process micro-heat stirring treatment, solid-liquid separation, and sintering.

[0008] Furthermore, one of the preparation methods of the polyphosphate and composite material comprises the following steps:

[0009] Step (1) putting an alkali metal source, a titanium source, a phosphorus source, a carbon source, water, and an acidic catalyst into a glass or enamel reactor;

[0010] Step (2) stirring the reaction mixture under heating conditions;

[0011] Step (3) separating the solid and liquid of the mixture after the reaction and drying it to obtain a powdery precursor for preparing the corresponding polyphosphate and composite material;

[0012] Step (4) calcining the precursor in an inert or air atmosphere, and obtaining the polyphosphate or polyphosphate composite material after natural cooling.

[0013] The titanium source is metatitanic acid.

[0014] The phosphorus source is phosphoric acid, dilithium phosphate, disodium phosphate or dipotassium phosphate.

[0015] The alkali metal source is dilithium phosphate, lithium citrate, lithium oxalate, lithium tartrate, lithium malate, disodium phosphate, sodium citrate, sodium oxalate, sodium tartrate, sodium malate, dipotassium phosphate, potassium citrate, potassium oxalate, potassium tartrate, and potassium malate.

[0016] The carbon source is lithium citrate, lithium oxalate, lithium tartrate, lithium malate, sodium citrate, sodium oxalate, sodium tartrate, sodium malate, potassium citrate, potassium oxalate, potassium tartrate, potassium malate, glucose, sucrose, carbon nanotubes, and graphene.

[0017] The molar ratio of the alkali metal element, the titanium element and the phosphorus element is 1:2:3, and the carbon source is 5%-15% of the theoretical output of the titanium phosphate salt.

[0018] The acid catalyst is an inorganic strong acid, and the amount used is 0.1%-2% of the mass of metatitanic acid.

[0019] Furthermore, when preparing the reaction mixture in step (1), an appropriate amount of water is added to control the solid content to be between 30% and 60%.

[0020] Furthermore, when preparing the reaction mixture in step (1), the acidic catalyst used is an inorganic strong acid such as sulfuric acid and nitric acid, and the amount used is 0.1%-2% of the mass of the metatitanic acid.

[0021] Furthermore, the heating temperature of step (2) is 80-100° C., the time is 2-10 hours, and the stirring method is mechanical at a rate of 60-300 rpm.

[0022] Furthermore, the solid-liquid separation method in step (3) is filtration, centrifugation, spray drying or direct drying, and the preferred method is filtration or spray drying.

[0023] Furthermore, the heating rate in step (4) is 5-20°C / min, and after heating to 350-450°C, the mixture is kept at this temperature and calcined for 120-480 minutes.

[0024] At present, the temperature required for solid phase synthesis of titanium phosphate is 750°C or above. The present invention prepares it at a low temperature of about 350-450°C, which has significant advantages.

[0025] Phosphoric acid is highly acidic and is a viscous liquid. It is difficult to process it with other raw materials into a powdery precursor with strong operability. Therefore, phosphoric acid is used as a raw material to realize the large-scale preparation of sodium titanium phosphate. In the present invention, all raw materials have undergone obvious chemical reactions after being treated in water and have a preliminary similar bonding form. This state is conducive to the conversion into sodium titanium phosphate products. The activation energy barrier that needs to be overcome is low, so the product can be generated at a lower temperature.

[0026] Figure 8 By comparing the infrared spectra of the raw material metatitanic acid and the precursor, it can be seen that after the reaction steps set by the present invention, the infrared of the precursor has undergone significant changes compared with metatitanic acid. -1The strong peak at about 779 cm is attributed to the vibration absorption of Ti-O bonds, but this strong peak basically disappears in the infrared spectrum of the precursor. -1 A weaker peak appears at the center, which is attributed to the absorption of the Ti-OP bond in the precursor, indicating that the raw materials such as titanic acid and phosphoric acid have undergone significant changes after treatment to form a new bonding form.

[0027] Fig. 9 The infrared spectra of the sodium titanium phosphate product and the precursor were compared. The two spectra are similar. The absorption peak in the product (1033 cm -1 ) compared to the precursor (1000 cm -1 ) has a slight blue shift, indicating that all the raw materials have undergone obvious chemical reactions after being treated in water and have a preliminary similar bonding form. This state is conducive to the conversion to sodium titanium phosphate products, and the activation energy barrier to be overcome is low, so the product can be generated at a lower temperature.

[0028] Beneficial effects of the present invention:

[0029] (1) The present invention provides a technical solution for preparing titanium phosphate salts with NASICON structure and composite materials thereof on a large scale using abundant and cheap metatitanic acid and phosphoric acid as raw materials. In the technical solution of the present invention, not only are the raw materials abundant and cheap, but also there are few by-products and no harmful gas emissions, which is environmentally friendly.

[0030] (2) The present invention provides a technical solution for preparing titanium phosphate salts with NASICON structure and composite materials thereof through activated intermediates. Using sulfuric acid as a catalyst, the starting raw materials are pre-reacted in water. During the reaction, the long chain of metatitanic acid insoluble in water is gradually cut off under the action of strong acid and bonds with phosphate to form a phosphate-titanium complex with a three-dimensional complex structure. This complex can make alkali metal elements, titanium and phosphate evenly mixed at the atomic level. In traditional solid phase synthesis, the ion diffusion of alkali metal elements and phosphate particles to titanium oxide particles is difficult and the diffusion distance is long. The energy to be overcome is high, so long-term high-temperature calcination is required to achieve it. The activated intermediate obtained by the treatment of the present invention is not only evenly mixed with the structural unit at the atomic level, but also the phosphate and titanium elements have partial bonding, so the preparation of the target product can be achieved at a lower temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 It is a diagrammatic representation of the high temperature solid phase synthesis mechanism and the synthesis mechanism of the activated intermediate of the present invention;

[0033] FIG2 is an XRD pattern of the activated precursor in Example 1;

[0034] FIG3 is an XRD pattern of LiTi2(PO4)3 prepared in Example 1;

[0035] FIG4 is an XRD pattern of the activated precursor in Example 2;

[0036] FIG5 is an XRD pattern of NaTi2(PO4)3 prepared in Example 2;

[0037] FIG6 is an XRD pattern of the activated precursor in Example 3;

[0038] FIG7 is an XRD pattern of KTi2(PO4)3 prepared in Example 3;

[0039] Figure 8 Infrared spectra of raw material metatitanic acid and precursor;

[0040] Fig. 9 Infrared spectra of sodium titanium phosphate products and precursors. Implementation

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0042] A method for preparing a lithium titanium phosphate material comprises the following steps:

[0043] (1) Add 200 ml of water, 52 g of lithium dihydrogen phosphate, 98 g of metatitanic acid, 230 g of phosphoric acid (85%), and 0.5 ml of concentrated sulfuric acid into a glass reactor in sequence;

[0044] (2) The reaction mixture was stirred and refluxed for 6 hours.

[0045] (3) The cooled reaction mixture is vacuum filtered to obtain a filter cake, which is then dried at 80°C to obtain an active precursor;

[0046] (4) The precursor is placed in a muffle furnace, heated to 300°C at a rate of 5°C / min, kept warm for 30 minutes, heated to 450°C at a rate of 10°C / min, calcined for 240 minutes, and naturally cooled to room temperature to obtain a pure phase of lithium titanium phosphate.

[0047] The XRD pattern of the activated precursor is as follows Figure 2 As shown, the activated precursor is not only evenly mixed with the structural unit at the atomic level, but also the phosphate and titanium elements have already partially bonded. During the reaction, the long chain of metatitanic acid that is insoluble in water is gradually cut off under the action of strong acid and bonds with the phosphate to form a phosphate-titanium complex with a three-dimensional complex structure. This complex can evenly mix alkali metal elements, titanium, and phosphate at the atomic level. The XRD spectrum of the prepared LiTi2(PO4)3 is shown in Figure 3 As shown, the diffraction peak completely corresponds to the pure phase LiTi2(PO4)3, the #PDF number is 35-0754, and no other impurity peaks are found, indicating that the prepared product has a high purity; at the same time, the diffraction peak intensity is high, indicating that the product has good crystallinity. Example 2

[0048] A method for preparing a sodium titanium carbon phosphate material comprises the following steps:

[0049] (1) Add 200 ml of water, 60 g of sodium dihydrogen phosphate, 98 g of titanic acid, 230 g of phosphoric acid (85%), and 0.5 ml of concentrated sulfuric acid into a glass reactor in sequence;

[0050] (2) stirring the reaction mixture and refluxing for 6 hours;

[0051] (3) The cooled reaction mixture is vacuum filtered to obtain a filter cake, which is then dried at 80°C to obtain an active precursor;

[0052] (4) The precursor was placed in a muffle furnace, heated to 300°C at a rate of 5°C / min, kept at this temperature for 30 minutes, heated to 400°C at a rate of 10°C / min, calcined for 120 minutes, and naturally cooled to room temperature to obtain a pure phase of sodium titanium phosphate.

[0053] The diffraction peak completely corresponds to the pure phase NaTi2(PO4)3, with the #PDF number being 33-1296, and no other impurity peaks are found, indicating that the prepared product has a high purity; at the same time, the diffraction peak intensity is high, indicating that the product has good crystallinity.

[0054] Example 3 A method for preparing a potassium titanium carbon phosphate material comprises the following steps:

[0055] (1) Add 200 ml of water, 68 g of potassium dihydrogen phosphate, 98 g of metatitanic acid, 345 g of phosphoric acid (85%), and 1.0 ml of concentrated sulfuric acid into a glass reactor in sequence;

[0056] (2) stirring the reaction mixture and refluxing for 9 hours;

[0057] (3) The cooled reaction mixture is vacuum filtered to obtain a filter cake, which is then dried at 80°C to obtain an active precursor;

[0058] (4) The precursor was placed in a muffle furnace, heated to 300°C at a rate of 5°C / min, kept at this temperature for 30 minutes, heated to 450°C at a rate of 10°C / min, calcined for 180 minutes, and naturally cooled to room temperature to obtain a pure phase of potassium titanium phosphate.

[0059] The diffraction peak completely corresponds to the pure phase KTi2(PO4)3, the #PDF number is 34-0131, and no other impurity peaks are found, indicating that the prepared product has a high purity; at the same time, the diffraction peak intensity is high, indicating that the product has good crystallinity.

[0060] Example 4 A method for preparing a carbon-coated sodium titanium carbon phosphate composite material comprises the following steps:

[0061] (1) Add 200 ml of water, 49 g of sodium citrate, 98 g of titanic acid, 345 g of phosphoric acid (85%), and 1.0 ml of concentrated sulfuric acid into a glass reactor in sequence;

[0062] (2) stirring the reaction mixture and refluxing for 9 hours;

[0063] (3) The cooled reaction mixture is vacuum filtered to obtain a filter cake, which is then dried at 80°C to obtain an active precursor;

[0064] (4) The precursor was placed in a muffle furnace, heated to 300°C at a rate of 5°C / min, kept at this temperature for 30 minutes, heated to 600°C at a rate of 10°C / min, calcined for 180 minutes, and naturally cooled to room temperature to obtain a carbon-coated sodium titanium phosphate material.

[0065] Example 5 A method for preparing a sodium titanium carbon phosphate / carbon nanotube composite material comprises the following steps:

[0066] (1) 200 ml of water, 60 g of sodium dihydrogen phosphate, 98 g of titanic acid, 345 g of phosphoric acid (85%), 1.0 ml of concentrated sulfuric acid, and 300 g of carbon nanotube aqueous dispersion (content of about 4%) were added to a glass reactor in sequence;

[0067] (2) stirring the reaction mixture and refluxing for 9 hours;

[0068] (3) The obtained reaction slurry is spray dried, and the air inlet temperature is controlled to be 180°C and the air outlet temperature is controlled to be 90°C to obtain a powdered active precursor;

[0069] (4) The precursor was placed in a muffle furnace, heated to 300°C at a rate of 5°C / min, kept at this temperature for 30 minutes, heated to 600°C at a rate of 10°C / min, calcined for 180 minutes, and naturally cooled to room temperature to obtain a sodium titanium phosphate / carbon nanotube composite material.

[0070] application:

[0071] The sodium titanium phosphate / carbon nanotube composite material prepared in Example 5 was used as an electrode material to assemble a sodium ion battery, and the electrochemical performance of the assembled sodium ion battery was tested;

[0072] Assembling a sodium-ion battery involves the following steps:

[0073] The carbon-coated sodium titanium phosphate composite material, a conductive agent (Super P) and a binder (polyvinylidene fluoride) are dissolved in N-methylpyrrolidone to obtain a coating slurry; the mass ratio of the carbon-coated sodium titanium phosphate composite material, the conductive agent and the binder is 7:2:1;

[0074] The obtained coating slurry was evenly applied on the copper foil, and then vacuum dried at 110°C for 2 hours and pressed using a roller press to obtain the negative electrode of the sodium ion battery; the loading on the copper foil was 1.5 mg / cm 2 ;

[0075] CR2032-type button cells were assembled in an argon-filled glove box using a metallic sodium sheet as the counter electrode and glass fiber as the separator. The electrolyte was 1 mol / L NaClO4 dissolved in a mixture of ethylene carbonate and dimethyl carbonate (1:1, v / v).

[0076] The electrochemical performance of the assembled sodium-ion battery was tested: constant current discharge / charge tests were performed using Land-2001A (Wuhan, China) at a voltage of 1.5-3 V. The specific capacity was 109 mAh / g at a 0.1C rate, 93 mAh / g at a 0.5C rate, and 75 mAh / g at a 1.0 C rate.

[0077] The above are preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing a titanium phosphate salt and a composite material having a NASICON structure, characterized in that: The steps include: (1) Putting an alkali metal source, a titanium source, a phosphorus source, a carbon source, water, and an acidic catalyst into a reaction kettle; (2) stirring the reaction mixture under heating conditions at a temperature of 80-100° C. for a period of 2-10 hours; (3) separating the solid and liquid of the reaction mixture and drying it to obtain a powdery precursor for preparing the corresponding polyphosphate and composite material; (4) calcining the precursor in an inert atmosphere or air, and obtaining the titanium phosphate salt and the composite material after natural cooling; The titanium source in step (1) is metatitanic acid; In step (1), the acidic catalyst is an inorganic strong acid, and the amount used is 0.1%-2% of the mass of metatitanic acid; The heating rate in step (4) is 5-20°C / min, and after heating to 350-450°C, the mixture is kept at this temperature and calcined for 120-480 minutes.

2. The method for preparing the titanium phosphate salt and composite material with NASICON structure according to claim 1, characterized in that: The phosphorus source is phosphoric acid, dilithium phosphate, disodium phosphate or dipotassium phosphate.

3. The method for preparing the titanium phosphate salt and composite material with NASICON structure according to claim 1, characterized in that: The alkali metal source is dilithium phosphate, lithium citrate, lithium oxalate, lithium tartrate, lithium malate, disodium phosphate, sodium citrate, sodium oxalate, sodium tartrate, sodium malate, dipotassium phosphate, potassium citrate, potassium oxalate, potassium tartrate, and potassium malate.

4. The method for preparing the titanium phosphate salt and composite material with NASICON structure according to claim 1, characterized in that: The carbon source is dilithium phosphate, lithium citrate, lithium oxalate, lithium tartrate, lithium malate, disodium phosphate, sodium citrate, sodium oxalate, sodium tartrate, sodium malate, dipotassium phosphate, potassium citrate, potassium oxalate, potassium tartrate, potassium malate, glucose, sucrose, carbon nanotubes, and graphene.

5. The method for preparing the titanium phosphate salt and composite material with NASICON structure according to claim 1, characterized in that: When preparing the reaction mixture in step (1), add an appropriate amount of water to control the solid content to 30%-60%.

6. The method for preparing the titanium phosphate salt and composite material with NASICON structure according to claim 1, characterized in that: The molar ratio of the alkali metal element, the titanium element and the phosphorus element is 1:2:3, and the carbon source is 5%-15% of the theoretical output of the titanium phosphate salt.

7. Titanium phosphate with NASICON structure prepared by the preparation method according to any one of claims 1 to 6.