A fiber-reinforced halogen-free flame-retardant nylon composition and preparation method thereof
Through the design of fiber reinforcement and specific component proportions, the flue gas and toxic gas problems of nylon materials during combustion are solved, and its flame retardant and mechanical properties are improved, achieving efficient application of halogen-free flame retardant nylon materials.
Patent Information
- Application Number
- CN202310394836.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-04-13
AI Technical Summary
Existing nylon materials produce a large amount of thick smoke and toxic and harmful gases when burned, and their flammability and poor notch impact performance limit their application range. The use of halogen-free flame retardant materials will lead to weakening of mechanical properties.
Using fiber-reinforced halogen-free flame retardant nylon compositions, including nylon resin, nanoboron fibers, phosphorus-containing flame retardant and hyperbranched polyols, the high-strength and good flame retardant properties are formed through specific component ratios and processes. Material.
The flame retardant modification and toughening of nylon materials are achieved, and the production of thick smoke and toxic gases during combustion is avoided. It takes into account strength performance and environmental protection and safety requirements, and the flame retardant level reaches UL94-V0 level.
Smart Images

Figure BDA0004177310500000111 
Figure BDA0004177310500000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nylon materials, and particularly relates to a fiber-reinforced halogen-free flame-retardant nylon composition and a preparation method thereof. Background Art
[0002] Nylon is a synthetic thermoplastic linear polyamide first produced by American chemist Wallace Carothers in 1935. It is usually referred to by the chemical name PA (such as PA 6 or PA 6 / 66). The most common colors are black, white and natural colors, including PA6, PA66, PA610, PA1010, etc., with high strength, high wear resistance and high chemical corrosion resistance. Nylon can be used in a variety of applications, including clothing, reinforcement materials for rubber materials such as tires, ropes, and plastic parts for vehicles and mechanical equipment. It has excellent strength, relatively good wear resistance and moisture absorption, long service life, chemical resistance, elasticity, easy cleaning, and is often used as a substitute for low-strength metals. Due to its good strength, heat resistance and chemical compatibility, it is also the preferred plastic for components in the engine compartment of vehicles.
[0003] Although nylon has a high melting point, it cannot withstand open flames well and is a flammable material. If exposed to open flames, it will easily burn. At the same time, its hygroscopic nature leads to poor notched impact performance, which limits the application of nylon. The usual practice is to combine with different materials to obtain different material properties. Nylon is flame-retardant modified and enhanced by adding flame retardants, elastomers and fibers. However, most flame retardants on the market are halogen flame retardants, which produce a lot of thick black smoke when burned, and also produce a lot of toxic and harmful gases.
[0004] Patent CN101250323A discloses a flame retardant and smoke suppression nylon 6 composite material, the raw material composition of which is calculated by weight: 100 parts of nylon 6, 0.5-10 parts of hydrotalcite, 10-40 parts of brominated flame retardant, 2-10 parts of antimony trioxide, and 0-35 parts of alkali-free glass fiber. Although the nylon 6 composite material can achieve a high flame retardant efficiency and a good smoke suppression effect, it is difficult to avoid the harm of a small amount of toxic smoke emitted to the human body.
[0005] Patent CN114031935A provides a flame retardant nylon material, which mainly includes the following components by mass: nylon resin 1: 10-35 parts; nylon resin 2: 10-35 parts; brominated polystyrene: 2-18 parts; polybrominated polystyrene: 2-18 parts; antimony trioxide: 2-8 parts; maleic anhydride grafted SEBS: 0-5 parts; maleic anhydride grafted POE: 0-5 parts; maleic anhydride grafted polyethylene: 0-5 parts; linear low-density polyethylene: 0-15 parts; polytetrafluoroethylene: 5-10 parts; nucleating agent: 0.1-0.4 parts; primary antioxidant: 0.1-0.4 parts; auxiliary antioxidant: 0.1-0.4 parts; lubricant: 0.3-0.8 parts; hydrolysis resistance agent: 0.1-0.4 parts; coupling agent: 0.5-1.5 parts. The flame-retardant nylon material has the characteristics of good flame retardancy and strong low-temperature resistance, and can adapt to various temperature environments. However, its raw material components contain a large amount of bromine-containing compounds. Once exposed to high temperatures, it is easy to produce toxic and harmful gases that pollute the environment and affect human health.
[0006] The structural increase plan for nylon is as follows:
[0007] CN113265722A discloses an ultra-high strength melt-blown nylon reinforced base material and its production process; the material is composed of the following raw materials in parts by weight: 60 to 100 parts of PA6, 10 to 30 parts of PA66, 10 to 30 parts of alkali-free short-cut glass fibers, 6 to 11 parts of nano-boron fibers, 8 to 16 parts of maleic anhydride grafted EPDM rubber, 20 to 40 parts of modified nano-mica powder, 4 to 8 parts of ethylene-propylene copolymer grafted maleic anhydride, 1.2 to 1.8 parts of antioxidant, 1.5 to 2.5 parts of dispersant and 1.0 to 3.0 parts of lubricant.
[0008] It can be seen that the use of solubilizers and fiber reinforcement to improve the strength of nylon is a commonly used technology in this field.
[0009] The use of halogen-free flame retardant materials can improve the fire retardant properties of nylon, but it will weaken the mechanical properties of nylon.
[0010] The use of hyperbranched polyols to prepare flame retardant materials is an emerging branch in this field, as shown in:
[0011] CN114685800A provides a phosphorus-containing hyperbranched polyol, a phosphorus-containing hyperbranched epoxy resin, a preparation method thereof, a composition and a cyanate resin. The phosphorus-containing hyperbranched polyol comprises any one or more of the following general structural formulas: wherein R1 is R2 is and / or wherein R5, R6, R9, R 10Each is independently selected from any one of H and C1-C3 alkyl, "*" in R1 is independently connected to hydroxyl or R2, and "*" in R2 is independently connected to one of hydroxyl, R1 and R2. When phosphorus-containing hyperbranched polyol is used to prepare phosphorus-containing hyperbranched epoxy resin, a large number of active groups such as hydroxyl groups exist on the highly branched molecular chain of phosphorus-containing hyperbranched epoxy resin, thereby improving the toughness, tensile strength, bending strength and flame retardancy of the resin system in the preparation of cyanate resin, thereby ensuring the mechanical properties while taking into account the flame retardancy of the resin system.
[0012] This scheme grafts phosphorus on hyperbranched polyol as a flame retardant material, which is the main component of the flame retardant material.
[0013] CN106750248B discloses a hyperbranched flame retardant polyether polyol and a preparation method thereof, wherein the hyperbranched flame retardant polyether polyol is an A2B3 type hyperbranched structure, and its structural formula is: wherein R is -CH3, -C6H5 or -O-C6H5; n is in the range of 5 to 100. The present invention firstly reacts phosphonyl chloride with trihydroxymethylphosphine oxide, and by controlling the ratio of the two, obtains a hyperbranched polyol with terminal hydroxyl groups by a monomer polycondensation method at 70°C to 110°C; then, the hyperbranched polyol is subjected to a ring-opening polymerization reaction with an epoxy compound, and finally obtains a novel hyperbranched flame retardant polyether polyol with a neutral pH and low viscosity.
[0014] This solution also involves phosphating the hyperbranched polyol to obtain a flame retardant material.
[0015] With the increasingly stringent requirements for environmental protection and safety, halogen-free and harmless materials will become the mainstream direction of the future market. Therefore, it is necessary to provide a reinforced and toughened halogen-free flame-retardant nylon material. Summary of the invention
[0016] In view of the shortcomings of the prior art, the first object of the present invention is to provide a fiber-reinforced and toughened halogen-free flame-retardant nylon material. The present invention provides a fiber-reinforced halogen-free flame-retardant nylon composition, which realizes flame-retardant modification and strengthening and toughening of nylon, and because of the use of halogen-free flame retardants, it avoids the generation of a large amount of thick black smoke or toxic and harmful gases during combustion, taking into account the requirements of strength performance and environmental safety.
[0017] The second object of the present invention is to provide a method for preparing the above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition.
[0018] In order to achieve the first object of the invention, the present invention adopts the following technical scheme: a fiber-reinforced halogen-free flame-retardant nylon composition, comprising the following components in parts by weight:
[0019] 90-100 parts of nylon resin mixture,
[0020] 20-30 parts of nano boron fiber,
[0021] Flame retardant 12-18 parts,
[0022] 10-15 parts of toughening agent,
[0023] 3 to 9 parts of compatibilizer,
[0024] The compatibilizer contains no less than 30% of hyperbranched polyol;
[0025] The flame retardant contains no less than 30% phosphorus-containing flame retardant and no less than 40% zinc borate.
[0026] The above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition includes the following components by weight:
[0027] 92-95 parts of nylon resin mixture,
[0028] 25-28 parts of nano boron fiber,
[0029] Flame retardant 12-14 parts,
[0030] 13-15 parts of toughening agent,
[0031] 4-6 parts of compatibilizer,
[0032] The compatibilizer contains 30-50% of hyperbranched polyol and 50%-70% of maleic anhydride modifier;
[0033] The flame retardant contains 30-40% of phosphorus-containing flame retardant and 60-70% of zinc borate.
[0034] In the above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition, the maleic anhydride modified substance is one or more of maleic anhydride grafted ABS, maleic anhydride grafted PE, maleic anhydride grafted EPDM, maleic anhydride grafted EVA, and maleic anhydride grafted POE.
[0035] In the above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition, the nylon resin mixture consists of nylon resin and POE; the nylon resin is a low-viscosity nylon resin with a viscosity of 2.2-2.8 Pa.S, preferably, the nylon resin is PA6, PA66, PA610 or PA1010;
[0036] The ratio of the nylon resin to POE is 40-60:10.
[0037] In the above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition, the diameter of the nano-boron fiber is 45-82 nm.
[0038] In the above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition, the phosphorus-containing flame retardant is one or more of black phosphorus, microcapsule-encapsulated red phosphorus, hypophosphite, hypophosphite, ammonium polyphosphate, diammonium phosphate, melamine polyphosphate, triphenyl phosphate, triethyl phosphate, triisopropylphenyl phosphate, trioctyl phosphate, tolyl diphenyl phosphonate, and melamine phosphate.
[0039] In the above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition, the toughening agent is one or more of polyethylene, ethylene-1-butene copolymer, ethylene-hexene copolymer and ethylene-methacrylic acid copolymer.
[0040] The above-mentioned fiber-reinforced halogen-free flame-retardant nylon composition also includes an antioxidant and a processing aid; the antioxidant is one or more of antioxidant 1098, hindered phenol antioxidants, and phosphite antioxidants; the processing aid is one or more of ethylene bisstearamide, polyester wax, magnesium stearate, calcium stearate, silicone oil, and white oil.
[0041] At the same time, the present invention also discloses a method for preparing the fiber-reinforced halogen-free flame-retardant nylon composition as described above, comprising the following steps:
[0042] (1) Weigh each component;
[0043] (2) adding the nylon resin mixture, flame retardant, toughening agent and compatibilizer into a high-speed mixer and mixing them thoroughly for 8 to 10 minutes to obtain a premix;
[0044] (3) placing the premix and nano-boron fiber into a twin-screw extruder for strip drawing, cooling, pelletizing and drying, wherein the screw diameter of the twin-screw extruder is 24-28 mm, and there are ten heating sections from the feed port to the die, and the temperatures of each section are 200-210° C., 220-240° C., 240-260° C., 240-260° C., 240-260° C., 240-260° C., 240-260° C., 210-230° C., 200-210° C. and 210-220° C.;
[0045] (4) Molding by injection molding or pressing process.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] First, the fiber-reinforced halogen-free flame-retardant nylon composition provided by the present invention has excellent mechanical properties such as tensile strength, flexural strength, flexural modulus, notched impact strength and good flame retardant properties, and the flame retardant grade reaches UL94-V0 level.
[0048] Second, the nano-boron fiber used in the present invention plays a role in greatly improving various mechanical properties of the nylon composition of the present invention, and the effect is remarkable. In actual use, it is found that compared with carbon fiber, nano-boron fiber can cooperate better with phosphorus flame retardant and zinc borate. The flame retardant is more inclined to form a carbonized layer on the surface of the nano-boron fiber to protect the fiber, so that the strength can be maintained when heated.
[0049] Third, the present invention adopts a nylon resin mixture of specific components. Compared with ordinary single nylon such as PA6 or a mixture of any two of the three components of the nylon resin mixture of the present invention, the mechanical properties and flame retardant properties of the product obtained under the action of other components of the present invention are better.
[0050] Fourthly, the flame retardant used in the present invention is a mixture of a phosphorus-containing flame retardant and zinc borate in a certain mass ratio, has a good flame retardant effect, and there is a synergistic effect between the phosphorus-containing flame retardant, zinc borate and hyperbranched polyol. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0052] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0053] Preparation of hyperbranched polyols Case 1
[0054] The preparation was carried out by referring to the preparation method of hyperbranched polyols described in "Study on Synthesis of Hyperbranched Polymers with Succinic Anhydride and Diethanolamine";
[0055] The polymer used in this case is not the esterification product in the study on the synthesis of hyperbranched polymers using succinic anhydride and diethanolamine, but a polyol intermediate.
[0056] The preparation steps are:
[0057] Weigh 4 g of diol amine and a certain amount of succinic anhydride in a molar ratio of 1, place in a three-necked flask, then use 30 mL of DMAc to dissolve it, and react with magnetic stirring at room temperature for 1 hour; add a small amount of catalyst p-toluenesulfonic acid and an appropriate amount (about 50 mL) of azeotropic water-carrying agent to the reaction system, stir and start to slowly heat the reaction until reflux occurs, continue to stir the reaction, condense and reflux the reaction phase through a water separator to separate the water produced by the reaction, and when no water droplets are generated, this step of the reaction is completed to obtain hyperbranched polyol 1.
[0058] Before being added to the subsequent examples, the hyperbranched polyol 1 solution was subjected to reduced pressure distillation to obtain a relatively viscous solution with a solid content of about 20-25%. The hyperbranched polyol described in the examples refers to the net content of the hyperbranched polyol.
[0059] Preparation of hyperbranched polyols Case 2
[0060] The process is similar to that in case 1, except that the molar ratio of diolamine to succinic anhydride is 1.1:1, and hyperbranched polyol 2 is obtained.
[0061] Preparation of hyperbranched polyols Case 3
[0062] The process is similar to that in case 1, except that the molar ratio of diolamine to succinic anhydride is 1.2:1, and hyperbranched polyol 3 is obtained.
[0063] Example 1
[0064] A fiber-reinforced halogen-free flame-retardant nylon composition comprises the following components in parts by weight:
[0065] 90 parts of nylon resin mixture,
[0066] 20 parts of nano boron fiber,
[0067] Flame retardant 12 parts,
[0068] 15 parts of toughening agent,
[0069] 3 parts of compatibilizer,
[0070] Antioxidant 0.1 part,
[0071] 3 parts of processing aid.
[0072] The flame retardant contains 35wt% black phosphorus and 65wt% zinc borate; the diameter of the nano boron fiber is 45-82nm;
[0073] The compatibilizer contains hyperbranched polyol 1 and POE-g-MAH (Dow Chemical, USA, GR216) in a weight ratio of 1:1;
[0074] The nylon resin mixture consists of nylon (Xinhui Meida PA6 M2500I) and POE (Dow Chemical, USA, POE8150) in a weight ratio of 58:10;
[0075] The toughening agent is polyethylene;
[0076] The processing aid is a mixture of silicone oil and white oil;
[0077] The antioxidant is 1098 (BASF Irganox 1098 from Germany);
[0078] The preparation method comprises the following steps:
[0079] (1) Weigh each component;
[0080] (2) adding the nylon resin mixture, flame retardant, toughening agent, compatibilizer, antioxidant and processing aid into a high-speed mixer and mixing them thoroughly for 10 minutes to obtain a premix;
[0081] (3) placing the premix and the nano-boron fiber into a twin-screw extruder for drawing, cooling, pelletizing, and drying, wherein the screw diameter of the twin-screw extruder is 24 mm, and there are ten heating sections from the feed port to the die, and the temperatures of each section are 200° C., 220° C., 240° C., 260° C., 240° C., 260° C., 240° C., 230° C., 200° C., and 210° C.;
[0082] (4) Molding by injection molding.
[0083] Example 2
[0084] The method is substantially the same as Example 1, except that the hyperbranched polyol is hyperbranched polyol 2.
[0085] Example 3
[0086] The method is substantially the same as Example 1, except that the hyperbranched polyol is hyperbranched polyol 3.
[0087] Example 4
[0088] The method is substantially the same as Example 1, except that the nylon resin is of type PA66 EPR27.
[0089] Example 5
[0090] The method is substantially the same as Example 1, except that the compatibilizer contains hyperbranched polyol 1 and POE-g-MAH (GR216, Dow Chemical, USA) in a weight ratio of 4:6.
[0091] Example 6
[0092] The method is substantially the same as Example 1, except that the compatibilizer contains hyperbranched polyol 1 and POE-g-MAH (GR216, Dow Chemical, USA) in a weight ratio of 3:7.
[0093] Example 7
[0094] It is substantially the same as Example 1, except that the flame retardant contains 30 wt % of black phosphorus and 70 wt % of zinc borate.
[0095] Example 8
[0096] It is substantially the same as Example 1, except that the flame retardant contains 40 wt % of black phosphorus and 60 wt % of zinc borate.
[0097] Example 9
[0098] The method is substantially the same as Example 1, except that the phosphorus-containing flame retardant is microcapsule-encapsulated red phosphorus.
[0099] Example 10
[0100] The method is substantially the same as Example 1, except that the phosphorus-containing flame retardant is triphenyl phosphate.
[0101] Embodiment 11
[0102] The process is substantially the same as in Example 1, except that the compatibilizer is hyperbranched polyol 1.
[0103] Comparative Example 1
[0104] The method is substantially the same as Example 1, except that the compatibilizer is POE-g-MAH (Dow Chemical, USA, GR216).
[0105] Comparative Example 2
[0106] The method is substantially the same as Example 1, except that the flame retardant is black phosphorus.
[0107] Comparative Example 3
[0108] The method is substantially the same as Example 1, except that the flame retardant is zinc borate.
[0109] Comparative Example 4
[0110] It is substantially the same as Example 1, except that the flame retardant is 35 wt % of black phosphorus and 65 wt % of aluminum hydroxide.
[0111] Comparative Example 5 (without flame retardant)
[0112] A fiber-reinforced halogen-free flame-retardant nylon composition comprises the following components in parts by weight:
[0113] 90 parts of nylon resin mixture,
[0114] 20 parts of nano boron fiber,
[0115] 15 parts of toughening agent,
[0116] 3 parts of compatibilizer,
[0117] Antioxidant 0.1 part,
[0118] 3 parts of processing aid.
[0119] Wherein, the diameter of the nano boron fiber is 45 to 82 nm;
[0120] The compatibilizer is POE-g-MAH (Dow Chemical, USA, GR216);
[0121] The nylon resin mixture consists of nylon (Xinhui Meida PA6 M2500I) and POE (Dow Chemical, USA, POE8150) in a weight ratio of 58:10;
[0122] The toughening agent is polyethylene;
[0123] The processing aid is a mixture of silicone oil and white oil;
[0124] The antioxidant is 1098 (BASF Irganox 1098 from Germany);
[0125] The preparation method comprises the following steps:
[0126] (1) Weigh each component;
[0127] (2) adding the nylon resin mixture, flame retardant, toughening agent, compatibilizer, antioxidant and processing aid into a high-speed mixer and mixing them thoroughly for 10 minutes to obtain a premix;
[0128] (3) placing the premix and the nano-boron fiber into a twin-screw extruder for drawing, cooling, pelletizing, and drying, wherein the screw diameter of the twin-screw extruder is 24 mm, and there are ten heating sections from the feed port to the die, and the temperatures of each section are 200° C., 220° C., 240° C., 260° C., 240° C., 260° C., 240° C., 230° C., 200° C., and 210° C.;
[0129] (4) Molding by injection molding.
[0130] Performance Testing
[0131] The nylon compositions prepared in Examples 1 to 11 and Comparative Examples 1 to 4 were tested for performance, wherein the flame retardancy was tested according to the UL94 standard, and the mechanical properties were tested according to the ISO standard, namely: tensile strength ISO 527-2, flexural strength and flexural modulus ISO 178, and notched impact strength ISO 180 / 1A. The test results are shown in Table 1.
[0132] Table 1
[0133]
[0134]
[0135] Result analysis:
[0136] 1. Through the analysis of Example 1 and Comparative Example 1 and Comparative Example 5, it can be seen that when only POE-g-MAH is added and no flame retardant is added, the mechanical properties of the board are the best; when POE-g-MAH and flame retardants (black phosphorus and zinc borate) are added, the mechanical properties are not as good as those when hyperbranched polyols are added. The possible reason is that hyperbranched polyols and PA can undergo a more sufficient chain extension reaction, so that the board is less mechanically damaged by the flame retardant; at the same time, compared with Comparative Example 1, Example 1 has better flame retardant properties, indicating that hyperbranched polyols help to better disperse the flame retardant before the chain extension reaction.
[0137] 2. By comparing Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, it can be found that the hyperbranched polyol of the present invention is more helpful for improving the dispersion performance of black phosphorus and zinc borate. On the one hand, it improves the flame retardant performance, and on the other hand, it reduces the influence of the flame retardant on the mechanical properties of the product.
[0138] The greatest contribution of the present invention is that it has been found that when a small amount of hyperbranched polyol is used, it can undergo a chain extension reaction with PA, thereby offsetting the effect of the flame retardant on the mechanical properties of PA and improving the flame retardant properties. Of course, the flame retardant properties of the present invention reaching the V0 level are not only caused by the flame retardant, PA and hyperbranched polyol, but are also closely related to the reasonable use of materials such as nano boron fibers.
[0139] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A fiber-reinforced halogen-free flame-retardant nylon composition, It is characterized in that It includes the following components by weight: 92~95 parts of nylon resin mixture, 25~28 parts of nano boron fiber, Flame retardant 12~14 parts, Toughener 13~15 parts, 4~6 parts of compatibilizer, The compatibilizer contains 30-50% of hyperbranched polyol and 50%-70% of maleic anhydride modification; The flame retardant contains 30-40% phosphorus-containing flame retardant and 60%-70% zinc borate; The maleic anhydride modified product is one or more of maleic anhydride grafted ABS, maleic anhydride grafted PE, maleic anhydride grafted EPDM, maleic anhydride grafted EVA, and maleic anhydride grafted POE; The nylon resin mixture consists of nylon resin and POE; the nylon resin is a low-viscosity nylon resin with a viscosity of 2.2-2.8 Pa.S; The ratio of the nylon resin to POE is 40-60:10; The diameter of the nano boron fiber is 45-82 nm.
2. A fiber-reinforced halogen-free flame-retardant nylon composition according to claim 1, It is characterized in that The phosphorus-containing flame retardant is one or more of black phosphorus, microcapsule-coated red phosphorus, hypophosphite, ammonium polyphosphate, diammonium phosphate, melamine polyphosphate, triphenyl phosphate, triethyl phosphate, triisopropylphenyl phosphate, trioctyl phosphate, tolyl diphenyl phosphonate, and melamine phosphate.
3. The fiber-reinforced halogen-free flame-retardant nylon composition according to claim 1, It is characterized in that The toughening agent is one or more of polyethylene, ethylene-1-butene copolymer, ethylene-hexene copolymer and ethylene-methacrylic acid copolymer.
4. The fiber-reinforced halogen-free flame-retardant nylon composition according to claim 1, It is characterized in that It also includes antioxidants and processing aids; the antioxidants are one or more of hindered phenol antioxidants and phosphite antioxidants; the processing aids are one or more of ethylene bisstearamide, magnesium stearate, calcium stearate, silicone oil, and white oil.
5. The fiber-reinforced halogen-free flame-retardant nylon composition according to claim 1, It is characterized in that The nylon resin is PA6, PA66, PA610 or PA1010.
6. A method for preparing the fiber-reinforced halogen-free flame-retardant nylon composition according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) Weigh each component; (2) Add the nylon resin mixture, flame retardant, toughening agent and compatibilizer into a high-speed mixer and mix thoroughly for 8 to 10 minutes to obtain a premix; (3) placing the premix and nano-boron fiber into a twin-screw extruder for drawing, cooling, pelletizing and drying, wherein the screw diameter of the twin-screw extruder is 24-28 mm, and there are ten heating sections from the feed port to the die, and the temperatures of each section are 200-210° C., 220-240° C., 240-260° C., 240-260° C., 240-260° C., 240-260° C., 240-260° C., 210-230° C., 200-210° C. and 210-220° C.; (4) Molding by injection molding or pressing process.