A preparation method of Li2TiO3 and a preparation method of lithium extraction adsorbent

Li2TiO3 was synthesized by calcining two-step solid-phase high-temperature method, and the lithium source was added in two steps to reduce the consumption of lithium source and the titanium dissolution rate, which solved the problem of high cost and insufficient stability of lithium ion sieve materials, and achieved low titanium dissolution of the material It has excellent adsorption performance, suitable for industrial production.

CN116409815BActive Publication Date: 2024-11-29BEIJING HUATEYUAN TECHNOLOGY CO LTD

Patent Information

Application Number
CN202211737926.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-11-29
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The high lithium source consumption of existing lithium ion sieves and excessive titanium dissolution rate leads to increased production costs and insufficient material stability, making it difficult to achieve large-scale industrial production.

Method used

Using a two-step solid-phase high-temperature calcination method, Li4Ti5O12 is first synthesized, and then reacted with the lithium source again to obtain Li2TiO3. By adding lithium sources in two steps, it can reduce the consumption of lithium sources and the titanium dissolution rate, and improve the structural stability and adsorption performance of the material. .

Benefits of technology

It effectively reduces lithium source consumption and titanium dissolution rate, simplifies the process flow, improves the low titanium dissolution and adsorption properties of the material, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116409815B_ABST
    Figure CN116409815B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of lithium extraction adsorbents, and in particular to a Li 2 TiO 3 Preparation method and preparation method of lithium extraction adsorbent. 2 TiO 3 The preparation method comprises the following steps: (a) dissolving an acid in water to obtain an acid solution; adding a lithium source to the acid solution and performing a first stirring to obtain a first mixed system; adding a titanium source to the first mixed system and performing a second stirring to obtain a second mixed system; drying, crushing and first calcining the second mixed system to obtain Li 4 Ti 5 O 12 ; (b) the Li 4 Ti 5 O 12 After being mixed with the lithium source, a second calcination is performed to obtain Li 2 TiO 3 The Li 2 TiO 3 The preparation method is to obtain the precursor Li by a two-step solid phase high temperature calcination method. 2 TiO 3 , which can effectively reduce lithium source consumption and titanium dissolution rate, is simple to operate, has a wide source of raw materials, and is easy to achieve large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium extraction adsorbents, and in particular to a method for preparing Li2TiO3 and a method for preparing a lithium extraction adsorbent. Background Art

[0002] In recent years, as an important component of power batteries, the demand for lithium has been rising. At present, the methods for extracting lithium from salt lake brine include precipitation, solvent extraction, nanofiltration, electrodialysis and adsorption. The adsorption method captures lithium ions through an adsorbent with high lithium ion selectivity, and then extracts lithium ions with an eluent, thereby achieving the purpose of separating lithium ions from other impurity ions. The adsorption method for extracting lithium has high production efficiency, no environmental pollution, and a mature and reliable process.

[0003] At present, the main types of lithium-ion-selective adsorbents are manganese oxide and titanium oxide. The adsorption rate of titanium-based lithium ion sieve is slower than that of manganese-based lithium ion sieve, but lithium titanium oxide has good mechanical strength, stable chemical properties, low titanium dissolution, good acid resistance, and better adsorption capacity than manganese-based lithium ion sieve. Combining the above advantages, titanium-based ion sieve has a better development prospect and is easier to realize industrialization. Ti in layered H2TiO3 titanium oxide lithium ion sieve in titanium-based ion sieve 4+ It has high stability, avoids disproportionation reaction and Jahn-Teller effect during lithium elution, has stable structure, excellent cycle performance and saturated adsorption capacity, and is a green and environmentally friendly lithium ion. It is obtained from the precursor Li2TiO3 after acid washing and is a research hotspot in titanium oxide lithium ion sieves.

[0004] The synthesis methods of precursor Li2TiO3 can be divided into solid phase method and liquid phase method (soft chemical method). The solid phase method mainly refers to high temperature solid phase method and microwave sintering method; the common liquid phase methods include sol-gel method (Sol-Gel), hydrothermal method, coprecipitation-crystallization method. The precursor prepared by soft chemical method has small particle size and uniform distribution, but there are problems such as complex process, expensive raw materials, and difficult process control, which is not conducive to industrialization. The solid phase method is simple in experimental operation, has a wide source of raw materials, and is suitable for mass production. It is one of the commonly used synthesis methods. Titanium dioxide or metatitanic acid is usually mixed with a lithium source and then calcined at high temperature to obtain the precursor Li2TiO3, but it is limited by the diffusion rate of the lithium source in the TiO2 crystal, and it takes a long time to sinter, resulting in the expensive lithium source. More than 5% excess is required to make up for the loss of lithium during the sintering process. There are problems such as high lithium source consumption and easy sintering of particles. In the acidification process of sintered particles, there is a phenomenon that the acidification rate is less than the dissolution rate, which leads to excessive titanium dissolution rate.

[0005] In view of the above technical shortcomings, the element doping method is currently used to modify Li2TiO3 to reduce lithium source consumption and titanium dissolution rate. However, the doping elements are mainly metals such as zirconium, cerium and iron, which increases the cost, and there is a risk of dissolution of doping elements during the acidification process.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] One aspect of the present invention relates to a method for preparing Li2TiO3, comprising the following steps:

[0008] (a) dissolving an acid in water to obtain an acid solution; adding a lithium source to the acid solution and performing a first stirring to obtain a first mixed system; adding a titanium source to the first mixed system and performing a second stirring to obtain a second mixed system; drying, crushing and performing a first calcination on the second mixed system to obtain Li4Ti5O 12 ;

[0009] (b) Li4Ti5O 12 After being mixed with the lithium source, a second calcination is performed to obtain Li2TiO3.

[0010] The preparation method of Li2TiO3 obtains the precursor Li2TiO3 by calcining in a two-step solid phase high temperature method, which can effectively reduce lithium source consumption and titanium dissolution rate, has simple operation, wide raw material sources, and is easy to realize large-scale production.

[0011] Another aspect of the present invention also relates to a method for preparing a lithium extraction adsorbent, comprising the following steps:

[0012] The Li2TiO3 prepared by the Li2TiO3 preparation method is acidified.

[0013] The lithium extraction adsorbent prepared by the method has very good low titanium dissolution performance during the acidification and adsorption processes, and also has excellent adsorption performance.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] (1) The preparation method of Li2TiO3 provided by the present invention is simple to operate, has a wide source of raw materials, and is easy to achieve large-scale production; the lithium source required for synthesizing Li2TiO3 is added in two steps, and the lithium source added in the first step is firstly synthesized with all the titanium sources into Li4Ti5O 12 , Li4Ti5O 12 In the crystal structure of Ti 4+It has a very stable extranuclear electronic structure, which makes it difficult to change its valence state. Therefore, before and after pickling and lithium extraction, the structure of other positions hardly changes, only the hydrogen ions and lithium ions are exchanged, so that the synthesized lithium extraction adsorbent has the characteristics of low titanium dissolution rate and good structural stability. In the second step, the remaining lithium source is added to Li4Ti5O 12 In the reaction synthesis of Li2TiO3, adding the lithium source in two steps (i.e. the principle of small amounts and multiple times) can effectively avoid the problem of too much lithium source added at one time, resulting in too low a diffusion rate when reacting with the titanium source. Adding a small amount of lithium source can accelerate the diffusion rate during the reaction, making the reaction more complete, and can solve the problem that due to the low diffusion rate, a long time of sintering is required, resulting in the expensive lithium source needing more than 5% excess to make up for the loss of lithium during the sintering process.

[0016] (2) The method for preparing the lithium extraction adsorbent provided by the present invention, the prepared lithium extraction adsorbent exhibits very good low titanium dissolution performance during the acidification and adsorption processes, and has excellent adsorption performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 Li4Ti5O provided in Example 1 of the present invention 12 SEM images;

[0019] Figure 2 This is a SEM image of the precursor Li2TiO3 provided in Example 1 of the present invention;

[0020] Figure 3 XRD diagram of Li2TiO3 precursor provided in Example 1 of the present invention;

[0021] Figure 4 Li4Ti5O provided in Example 2 of the present invention 12 SEM images;

[0022] Figure 5 This is a SEM image of the precursor Li2TiO3 provided in Example 2 of the present invention;

[0023] Figure 6 This is the XRD diagram of the precursor Li2TiO3 provided in Example 2 of the present invention. DETAILED DESCRIPTION

[0024] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0025] One aspect of the present invention relates to a method for preparing Li2TiO3, comprising the following steps:

[0026] (a) dissolving an acid in water to obtain an acid solution; adding a lithium source to the acid solution and performing a first stirring to obtain a first mixed system; adding a titanium source to the first mixed system and performing a second stirring to obtain a second mixed system; drying, crushing and performing a first calcination on the second mixed system to obtain Li4Ti5O 12 ;

[0027] (b) Li4Ti5O 12 After being mixed with the lithium source, a second calcination is performed to obtain Li2TiO3.

[0028] The preparation method of Li2TiO3 is to add the lithium source required for synthesizing Li2TiO3 in two steps. The lithium source added in the first step is firstly synthesized with all the titanium sources into Li4Ti5O 12 , Li4Ti5O 12 In the crystal structure of Ti 4+ It has a very stable extranuclear electronic structure, which makes it difficult to change its valence state. Therefore, before and after pickling and lithium extraction, the structure of other positions hardly changes, only the hydrogen ions and lithium ions are exchanged, so that the synthesized lithium extraction adsorbent has the characteristics of low titanium dissolution rate and good structural stability. In the second step, the remaining lithium source is added to Li4Ti5O 12 In the reaction synthesis of Li2TiO3, adding the lithium source in two steps (i.e. the principle of small amounts and multiple times) can effectively avoid the problem of too much lithium source added at one time, resulting in too low a diffusion rate when reacting with the titanium source. Adding a small amount of lithium source can accelerate the diffusion rate during the reaction, making the reaction more complete, and can solve the problem that due to the low diffusion rate, a long time of sintering is required, resulting in the expensive lithium source needing more than 5% excess to make up for the loss of lithium during the sintering process.

[0029] Preferably, in step (a), the molar ratio of the acid, the lithium source and the titanium source is 3-5:5-7:14-16 (eg, 3:7:14, 4:6:15 or 5:5:16).

[0030] Preferably, in step (a), the mass ratio of the total mass of the acid, the lithium source and the titanium source to the water is 1:(1-2) (eg, 1:1, 1:1.5 or 1:2).

[0031] Preferably, in step (b), the Li4Ti5O 12 The molar ratio of the lithium source is 0.5-1.5:2-4 (eg, 0.5:4, 1:3, 1.5:2).

[0032] Preferably, the first stirring speed is 120-200 rpm / min (e.g., 120 rpm / min, 130 rpm / min, 140 rpm / min, 150 rpm / min, 160 rpm / min, 170 rpm / min, 180 rpm / min, 190 rpm / min or 200 rpm / min).

[0033] Preferably, the first stirring time is 2 to 8 h (eg, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h or 8 h).

[0034] Preferably, the second stirring speed is 150-250 rpm / min (eg, 150 rpm / min, 170 rpm / min, 190 rpm / min, 210 rpm / min, 230 rpm / min or 250 rpm / min).

[0035] Preferably, the second stirring time is 1 to 2 h (eg, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h).

[0036] Preferably, the drying temperature is 110-180°C (eg, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C).

[0037] Preferably, the second mixed system is dried and crushed to a particle size of less than 150 μm (eg, 150 μm, 140 μm, 130 μm, 120 μm, 110 μm, 50 μm, 30 μm or 10 μm).

[0038] Preferably, the temperature of the first calcination is 700-850°C (e.g., 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C or 850°C).

[0039] Preferably, the first calcination time is 6 to 10 h (eg, 6 h, 7 h, 8 h, 9 h or 10 h).

[0040] Preferably, the heating rate of the first calcination is 5 to 20°C / min (eg, 5°C / min, 7°C / min, 9°C / min, 11°C / min, 13°C / min, 15°C / min, 17°C / min or 20°C / min).

[0041] Preferably, the second calcination temperature is 650-800°C (eg, 650°C, 660°C, 670°C, 690°C, 710°C, 720°C, 730°C, 750°C, 770°C, 790°C or 800°C).

[0042] Preferably, the second calcination time is 4 to 8 h (eg, 4 h, 5 h, 6 h, 7 h or 8 h).

[0043] Preferably, the heating rate of the second calcination is 10-20°C / min (eg, 10°C / min, 12°C / min, 14°C / min, 16°C / min, 18°C / min or 20°C / min).

[0044] Preferably, the acid solution comprises at least one of citric acid, acetic acid or oxalic acid.

[0045] Preferably, the lithium source includes at least one of lithium carbonate, lithium hydroxide or lithium chloride.

[0046] Preferably, the titanium source includes: titanium dioxide and / or metatitanic acid.

[0047] Another aspect of the present invention also relates to a method for preparing a lithium extraction adsorbent, comprising the following steps:

[0048] The Li2TiO3 prepared by the Li2TiO3 preparation method is acidified.

[0049] The method for preparing the lithium extraction adsorbent shows very good low titanium dissolution performance during the acidification and adsorption processes, and also has excellent adsorption performance.

[0050] Preferably, the acidification specifically comprises:

[0051] The Li2TiO3 is added to 50-60°C water at a solid-liquid ratio of 1: (3-20), and stirred evenly to form a slurry. Hydrochloric acid with a mass fraction of 16% to 18% is added dropwise to the slurry. When the pH of the slurry stabilizes at 2.0 to 2.3, the addition of hydrochloric acid is stopped.

[0052] Preferably, the acid used for acidification includes at least one of hydrochloric acid, nitric acid or sulfuric acid.

[0053] The embodiments of the present invention will be described in detail below with reference to specific examples and comparative examples.

[0054] Example 1

[0055] (1)Li4Ti5O 12 Preparation: Weigh a certain mass of raw materials according to the molar ratio of citric acid: lithium carbonate: nano titanium dioxide = 4:6:15, and calculate the water consumption according to the solid-liquid ratio of 1:1. First, slowly add citric acid to water, stirring while adding until the citric acid solid is completely dissolved in water, and then slowly and repeatedly add lithium carbonate in small amounts. This process will produce a large number of bubbles, which require vigorous stirring to accelerate defoaming. After all the lithium carbonate is added, continue stirring for 4 hours until the lithium carbonate is completely dissolved. Finally, add nano titanium dioxide powder and stir for 2 hours to make the titanium dioxide evenly dispersed without obvious granularity to obtain a uniformly dispersed solid-liquid mixture. The above-mentioned uniformly dispersed solid-liquid mixture is placed in an ordinary drying oven, dried at 110°C, crushed to a particle size of less than 150μm, and then placed in a muffle furnace for calcination at 800°C for 6 hours, and the heating rate is controlled to be 5°C / min, and finally Li4Ti5O 12 , set aside. Take a small amount of Li4Ti5O 12 For SEM characterization, the results are as follows Figure 1 shown.

[0056] (2) Preparation of Li2TiO3: According to the molar ratio of Li4Ti5O 12 :Lithium carbonate = 1:3 Weigh a certain mass of Li4Ti5O 12 and lithium carbonate, stir and mix them at high speed for 1-2 minutes, put them into a muffle furnace and roast them at 650℃ for 8 hours, control the heating rate to 10℃ / min, and obtain H2TiO3 precursor Li2TiO3, grind it into powder and set aside. Take a small amount of precursor Li2TiO3 for XRD and SEM characterization, the results are as follows Figure 2 and Figure 3 shown.

[0057] (3) Li2TiO3 acidification: The water volume is in a solid-liquid ratio of 1:5, and the prepared Li2TiO3 for lithium extraction is added to 50°C water, and stirred evenly under this temperature condition to form a slurry, and 16% hydrochloric acid is added dropwise to control the pH of the slurry at 2.0-2.3 until the pH does not rise (or rises very slowly), centrifuge and wash with water 2-4 times until the centrifugal supernatant TDS is less than 50mg / L, repeat the above acid washing steps twice, and finally dry in a 60°C oven to constant weight, and grind evenly after the temperature drops to room temperature to obtain the lithium extraction adsorbent H2TiO3 for use. Take a sample of the supernatant after each acidification to determine the concentration of Li and Ti therein, and the results are shown in Table 1.

[0058] (4) Preparation of test solution: Weigh lithium carbonate (1.60 g), sodium bicarbonate (7.61 g), anhydrous sodium sulfate (10.58 g), anhydrous sodium carbonate (11.86 g) and sodium chloride (78.31 g), dissolve in water and make up to 1 L, shake well and set aside.

[0059] Take the above test solution, add H2TiO3 according to the feed-to-solid ratio of 5g / L, stir the test under room temperature, and take samples at regular intervals to determine the concentrations of Li and Ti in the samples. The test results are shown in Table 2.

[0060] Table 1 Data table of lithium analysis and titanium dissolution during Li2TiO3 acidification process in Example 1

[0061] Acidification times Li in analytical solution (mg / L) Ti in analytical solution (mg / L) 1 9581.53 0.05 2 182.04 0.16 3 23.72 0.12

[0062] Table 2 Results of lithium adsorption and titanium dissolution of H2TiO3 over time in Example 1

[0063] Stirring time (h) Li(mg / L) Ti(mg / L) Li adsorption amount (mg / g) 0 297.41 0 0 1 159.32 0.15 27.62 3 135.98 0.34 32.28 24 98.96 0.42 39.69 48 93.38 0.41 40.80

[0064] Depend on Figure 1 and Figure 2 It can be seen that Li4Ti5O 12 The morphology is slightly different from that of the precursor Li2TiO3, indicating that the addition of the lithium source twice has no effect on the microscopic morphology of the prepared sample. The prepared precursor Li2TiO3 is granular and has a dense structure. Although there is particle agglomeration, the particle size distribution is generally <1μm. The small particle size and large specific surface area are conducive to the rapid adsorption and desorption of lithium.

[0065] Depend on Figure 3 It can be seen that in the XRD diagram, the precursor Li2TiO3 sample has strong characteristic diffraction peaks near 2θ of 18.48°, 20.22°, 35.94°, 43.72° and 63.5°, indicating that monoclinic Li2TiO3 has been synthesized.

[0066] It can be seen from Table 1 that during the acidification process, as the number of acidification times increases, Li in the precursor Li2TiO3 is extracted, but the concentration of Ti in the analytical solution is always less than 0.2 mg / L. At the same time, it can be seen from Table 2 that the lithium adsorption capacity of H2TiO3 obtained after acidification in a multi-ion mixed solution increases with time, and after about 24 hours of testing, it basically reaches the adsorption equilibrium state, the lithium adsorption amount is about 40 mg / g, and the Ti concentration in the test solution is less than 0.5 mg / g. In summary, the prepared lithium extraction adsorbent exhibits very good low titanium dissolution performance during both acidification and adsorption.

[0067] Example 2

[0068] (1)Li4Ti5O 12Preparation: Weigh a certain mass of raw materials according to the molar ratio of citric acid: lithium carbonate: nano titanium dioxide = 4:6:15, and calculate the water consumption according to the solid-liquid ratio of 1:2. First, slowly add citric acid to water, stirring while adding until the citric acid solid is completely dissolved in water, and then slowly and repeatedly add lithium carbonate in small amounts. This process will produce a large number of bubbles, which require vigorous stirring to accelerate defoaming. After all the lithium carbonate is added, continue stirring for 2 hours until the lithium carbonate is completely dissolved. Finally, add nano titanium dioxide powder and stir for 1 hour to make the titanium dioxide evenly dispersed without obvious particles to obtain a uniformly dispersed solid-liquid mixture. The above-mentioned uniformly dispersed solid-liquid mixture is placed in an ordinary drying oven, dried at 140°C, crushed to a particle size of less than 150μm, and then placed in a muffle furnace for calcination at 850°C for 6 hours, and the heating rate is controlled to be 20°C / min, and finally Li4Ti5O 12 , set aside. Take a small amount of Li4Ti5O 12 For SEM characterization, the results are as follows Figure 4 shown.

[0069] (2) Preparation of Li2TiO3: According to the molar ratio of Li4Ti5O 12 :Lithium carbonate = 1:3 Weigh a certain mass of Li4Ti5O 12 and lithium carbonate, stir and mix them at high speed for 1-2 minutes, put them into a muffle furnace and roast them at 750℃ for 4 hours, control the heating rate to 15℃ / min, and obtain H2TiO3 precursor Li2TiO3, grind it into powder and set aside. Take a small amount of precursor Li2TiO3 for XRD and SEM characterization, the results are as follows Figure 5 and Figure 6 shown.

[0070] (3) Li2TiO3 acidification: The water volume is in a solid-liquid ratio of 1:20, and the prepared Li2TiO3 for lithium extraction is added to 60°C water, and stirred evenly under this temperature condition to form a slurry, and 18% hydrochloric acid is added dropwise, and the pH of the slurry is controlled at 2.0-2.3 until the pH does not rise (or rises very slowly), and centrifuged and washed with water 2-4 times until the centrifuged supernatant TDS is less than 50mgL, and the above acid washing steps are repeated twice, and finally dried in an oven at 80°C to constant weight, and after the temperature drops to room temperature, it is ground evenly to obtain the lithium extraction adsorbent H2TiO3 for use. The supernatant samples after each acidification are taken to determine the concentrations of Li and Ti therein, and the results are shown in Table 3.

[0071] The adsorption test solution and test process of H2TiO3 are the same as those in Example 1. The results are shown in Table 4.

[0072] Table 3 Data of lithium analysis and titanium dissolution during Li2TiO3 acidification process in Example 2

[0073]

[0074] Table 4 Results of lithium adsorption and titanium dissolution of H2TiO3 over time

[0075] Stirring time (h) Li(mg / L) Ti(mg / L) Li adsorption amount (mg / g) 0 296.06 0 0 1 179.83 0.06 23.25 3 137.45 0.13 31.72 24 106.71 0.29 37.87 48 100.54 0.31 39.10

[0076] Depend on Figure 5 and Figure 6 It can be seen that Li4Ti5O 12 The morphology is slightly different from that of the precursor Li2TiO3, indicating that the addition of the lithium source twice has no effect on the microscopic morphology of the prepared sample. The prepared precursor Li2TiO3 is granular and has a dense structure. Although there is particle agglomeration, the particle size distribution is generally <1μm. The small particle size and large specific surface area are conducive to the rapid adsorption and desorption of lithium.

[0077] Depend on Figure 6 It can be seen that in the XRD diagram, the precursor Li2TiO3 sample has strong characteristic diffraction peaks near 2θ of 18.48°, 20.22°, 35.94°, 43.72° and 63.5°, indicating that monoclinic Li2TiO3 has been synthesized.

[0078] It can be seen from Table 3 that during the acidification process, as the number of acidification times increases, Li in the precursor Li2TiO3 is extracted, but the concentration of Ti in the analytical solution is always less than 0.3 mg / L. At the same time, it can be seen from Table 4 that the lithium adsorption capacity of H2TiO3 obtained after acidification in a multi-ion mixed solution increases with time, and basically reaches the adsorption equilibrium state after about 24 hours of testing, with a lithium adsorption amount of about 38 mg / g, and the Ti concentration in the test solution is less than 0.5 mg / g. In summary, the prepared lithium extraction adsorbent exhibits very good low titanium dissolution performance during both acidification and adsorption.

[0079] Comparative Example 1

[0080] (1)Li4Ti5O 12 Preparation: Weigh a certain mass of raw materials according to the molar ratio of citric acid: lithium carbonate: nano titanium dioxide = 2:3:3, and calculate the water consumption according to the solid-liquid ratio of 1:1. First, slowly add citric acid to water, stirring while adding until the citric acid solid is completely dissolved in water, and then slowly and repeatedly add lithium carbonate in small amounts. This process will produce a large number of bubbles, which need to be stirred vigorously to accelerate defoaming. After all the lithium carbonate is added, continue to stir for 4 hours until the lithium carbonate is completely dissolved. Finally, add nano titanium dioxide powder and stir for 2 hours to make the titanium dioxide evenly dispersed without obvious granularity to obtain a uniformly dispersed solid-liquid mixture. The above-mentioned uniformly dispersed solid-liquid mixture is placed in an ordinary drying oven, dried at 110°C, crushed to a particle size of less than 150μm, and then placed in a muffle furnace for calcination at 800°C for 6 hours, and the heating rate is controlled to be 5°C / min to obtain the H2TiO3 precursor Li2TiO3, which is ground into powder for use.

[0081] (2) Li2TiO3 acidification: The water volume is in a solid-liquid ratio of 1:5, and the prepared Li2TiO3 for lithium extraction is added to 50°C water, stirred evenly under this temperature condition to form a slurry, and 16% hydrochloric acid is added dropwise to control the pH of the slurry at 2.0-2.3 until the pH does not rise (or rises very slowly), centrifuged and washed with water 2-4 times until the TDS of the centrifuged supernatant is less than 50mg / L, and the above acid washing steps are repeated twice, and finally dried in a 60°C oven to constant weight, and ground evenly after the temperature drops to room temperature, to obtain the lithium extraction adsorbent H2TiO3 for use. The supernatant samples after each acidification are taken to determine the concentrations of Li and Ti therein, and the results are shown in Table 5.

[0082] The adsorption test solution and test process of H2TiO3 are the same as those in Example 1. The results are shown in Table 6.

[0083] Table 5 Comparative Example 1 Li2TiO3 Acidification Process Lithium Analysis and Titanium Dissolution Data

[0084] Acidification times Li in analytical solution (mg / L) Ti in analytical solution (mg / L) 1 8494.71 2.65 2 223.45 5.78 3 19.88 7.53

[0085] Table 6 Comparative Example 1 Lithium adsorption and titanium dissolution of H2TiO3 over time

[0086] Stirring time (h) Li(mg / L) Ti(mg / L) Li adsorption amount (mg / g) 0 230.47 0 0 1 182.53 1.82 9.58 3 147.85 2.26 16.52 24 133.24 6.67 19.44 48 122.51 7.02 21.59

[0087] It can be seen from Table 5 that during the acidification process, as the number of acidification times increases, Li in the precursor Li2TiO3 is extracted, and the concentration of Ti in the analytical solution is 2.65-7.53 mg / g, which increases significantly and is much higher than 0.3 mg / L. At the same time, it can be seen from Table 6 that the lithium adsorption capacity of H2TiO3 obtained after acidification in a multi-ion mixed solution increases with time, and basically reaches the adsorption equilibrium state at about 48 hours of the test, with a lithium adsorption amount of about 22 mg / g, while the Ti concentration in the test solution is as high as 7.02 mg / g. In summary, the lithium extraction adsorbent prepared by adding a lithium source once shows very high titanium dissolution performance during the acidification and adsorption processes, and the effect is far inferior to that of step-by-step addition of the lithium source, indicating that step-by-step addition of the lithium source has better technical effects.

[0088] Comparative Example 2

[0089] (1)Li4Ti5O 12Preparation: Weigh a certain mass of raw materials according to the molar ratio of citric acid: lithium carbonate: nano titanium dioxide = 4:6:15, and calculate the water consumption according to the solid-liquid ratio of 1:1. First, slowly add citric acid to water, stirring while adding until the citric acid solid is completely dissolved in water, and then slowly and repeatedly add lithium carbonate in small amounts. This process will produce a large number of bubbles, which require vigorous stirring to accelerate defoaming. After all the lithium carbonate is added, continue stirring for 4 hours until the lithium carbonate is completely dissolved. Finally, add nano titanium dioxide powder and stir for 2 hours to make the titanium dioxide evenly dispersed without obvious granularity to obtain a uniformly dispersed solid-liquid mixture. The above-mentioned uniformly dispersed solid-liquid mixture is placed in an ordinary drying oven, dried at 110°C, crushed to a particle size of less than 150μm, and then placed in a muffle furnace for roasting at 1050°C for 6 hours, and the heating rate is controlled to be 5°C / min, and finally Li4Ti5O 12 ,spare.

[0090] (2) Preparation of Li2TiO3: According to the molar ratio of Li4Ti5O 12 :Lithium carbonate = 1:3 Weigh a certain mass of Li4Ti5O 12 and lithium carbonate, stir the two at high speed for 1-2 minutes, put them into a muffle furnace and calcine at 1050°C for 8 hours, control the heating rate at 10°C / min, to obtain H2TiO3 precursor Li2TiO3, grind it into powder and set aside.

[0091] (3) Li2TiO3 acidification: The water volume is in a solid-liquid ratio of 1:5, and the prepared Li2TiO3 for lithium extraction is added to 50°C water, and stirred evenly under this temperature condition to form a slurry, and 16% hydrochloric acid is added dropwise to control the pH of the slurry at 2.0-2.3 until the pH does not rise (or rises very slowly), centrifuge and wash with water 2-4 times until the centrifugal supernatant TDS is less than 50mg / L, repeat the above acid washing steps twice, and finally dry in a 60°C oven to constant weight, and grind evenly after the temperature drops to room temperature to obtain the lithium extraction adsorbent H2TiO3 for use. Take a sample of the supernatant after each acidification to determine the concentration of Li and Ti therein, and the results are shown in Table 7.

[0092] The H2TiO3 adsorption test solution and test process are the same as in Example 1. The results are shown in Table 8.

[0093] Table 7 Comparative Example 2 Li2TiO3 Acidification Process Lithium Analysis and Titanium Dissolution Data

[0094] Acidification times Li in analytical solution (mg / L) Ti in analytical solution (mg / L) 1 5643.15 1.23 2 97.39 4.54 3 10.64 5.92

[0095] Table 8 Comparative Example 2 H2TiO3 lithium adsorption and titanium dissolution over time results

[0096] Stirring time (h) Li(mg / L) Ti(mg / L) Li adsorption amount (mg / g) 0 229.51 0 0 1 219.22 1.35 2.05 3 177.05 3.01 10.49 24 153.43 3.68 15.21 48 149.79 4.53 15.94

[0097] It can be seen from Table 7 that during the acidification process, as the number of acidification times increases, Li in the precursor Li2TiO3 is extracted, and the concentration of Ti in the analytical solution is 1.23-5.92 mg / g, which increases significantly and is much higher than 0.3 mg / L. At the same time, it can be seen from Table 8 that the lithium adsorption capacity of the H2TiO3 obtained after acidification in the multi-ion mixed solution increases with time, and basically reaches the adsorption equilibrium state after about 48 hours of testing, with a lithium adsorption amount of about 16 mg / g, while the Ti concentration in the test solution is as high as 4.53 mg / g. In summary, the lithium extraction adsorbent prepared at a calcination temperature of 1050°C exhibits very high titanium dissolution performance during the acidification and adsorption processes, and the effect is far inferior to that of Examples 1 and 2, indicating that better technical effects can be obtained by controlling a suitable calcination temperature.

[0098] Comparative Example 3

[0099] (1)Li4Ti5O 12 Preparation: Weigh a certain mass of raw materials according to the molar ratio of citric acid: lithium carbonate: nano titanium dioxide = 4:6:15, and calculate the water consumption according to the solid-liquid ratio of 1:1. First, slowly add citric acid to water, stirring while adding until the citric acid solid is completely dissolved in water, and then slowly and repeatedly add lithium carbonate in small amounts. This process will produce a large number of bubbles, which require vigorous stirring to accelerate defoaming. After all the lithium carbonate is added, continue stirring for 4 hours until the lithium carbonate is completely dissolved. Finally, add nano titanium dioxide powder and stir for 2 hours to make the titanium dioxide evenly dispersed without obvious granularity to obtain a uniformly dispersed solid-liquid mixture. The above-mentioned uniformly dispersed solid-liquid mixture is placed in an ordinary drying oven, dried at 110°C, crushed to a particle size of less than 150μm, and then placed in a muffle furnace for calcination at 500°C for 6 hours, and the heating rate is controlled to be 5°C / min, and finally Li4Ti5O 12 ,spare.

[0100] (2) Preparation of Li2TiO3: According to the molar ratio of Li4Ti5O 12 :Lithium carbonate = 1:3 Weigh a certain mass of Li4Ti5O 12 and lithium carbonate, stir the two at high speed for 1-2 minutes, put them into a muffle furnace and calcine at 500°C for 8 hours, control the heating rate at 10°C / min, to obtain H2TiO3 precursor Li2TiO3, grind it into powder and set aside.

[0101] (3) Li2TiO3 acidification: The water volume is in a solid-liquid ratio of 1:5, and the prepared Li2TiO3 for lithium extraction is added to 50°C water, and stirred evenly under this temperature condition to form a slurry, and 16% hydrochloric acid is added dropwise to control the pH of the slurry at 2.0-2.3 until the pH does not rise (or rises very slowly), centrifuge and wash with water 2-4 times until the centrifugal supernatant TDS is less than 50mg / L, repeat the above acid washing steps twice, and finally dry in a 60°C oven to constant weight, and grind evenly after the temperature drops to room temperature to obtain the lithium extraction adsorbent H2TiO3 for use. Take a sample of the supernatant after each acidification to determine the concentration of Li and Ti therein, and the results are shown in Table 9.

[0102] The H2TiO3 adsorption test solution and test process are the same as in Example 1. The results are shown in Table 10.

[0103] Table 9 Comparative Example 3 Li2TiO3 Acidification Process Lithium Analysis and Titanium Dissolution Data

[0104] Acidification times Li in analytical solution (mg / L) Ti in analytical solution (mg / L) 1 6533.27 3.63 2 150.14 6.85 3 20.59 7.79

[0105] Table 10 Comparative Example 3 Lithium adsorption and titanium dissolution of H2TiO3 over time

[0106] Stirring time (h) Li(mg / L) Ti(mg / L) Li adsorption amount (mg / g) 0 231.36 0 0 1 208.66 6.55 4.54 3 166.49 6.89 12.97 24 142.87 9.87 17.69 48 139.23 10.38 18.42

[0107] It can be seen from Table 9 that during the acidification process, as the number of acidification times increases, Li in the precursor Li2TiO3 is extracted, and the concentration of Ti in the analytical solution is 3.63-7.79 mg / g, which increases significantly and is much higher than 0.3 mg / L. At the same time, it can be seen from Table 10 that the lithium adsorption capacity of the H2TiO3 obtained after acidification in the multi-ion mixed solution increases with time, and basically reaches the adsorption equilibrium state after about 48 hours of testing, with a lithium adsorption amount of about 18 mg / g, while the Ti concentration in the test solution is as high as 10.38 mg / g. In summary, the lithium extraction adsorbent prepared at a calcination temperature of 500°C shows very high titanium dissolution performance during the acidification and adsorption processes, and the effect is far inferior to that of Examples 1 and 2, indicating that better technical effects can be obtained by controlling a suitable calcination temperature.

[0108] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A method for preparing Li2TiO3, characterized in that: The following steps are involved: (a) dissolving an acid in water to obtain an acid solution; adding a lithium source to the acid solution and performing a first stirring to obtain a first mixed system; adding a titanium source to the first mixed system and performing a second stirring to obtain a second mixed system; The second mixed system is dried, crushed and first calcined to obtain Li4Ti5O 12 ; The temperature of the first calcination is 700-850°C; (b) Li4Ti5O 12 After being mixed with the lithium source, a second calcination is performed to obtain Li2TiO3; The second calcination temperature is 650-800°C.

2. The method for preparing Li2TiO3 according to claim 1, characterized in that: In step (a), the molar ratio of the acid, the lithium source and the titanium source is 3-5:5-7:14-16.

3. The method for preparing Li2TiO3 according to claim 1, characterized in that: In step (a), the mass ratio of the total mass of the acid, the lithium source and the titanium source to the mass of the water is 1:(1-2).

4. The method for preparing Li2TiO3 according to claim 1, characterized in that: In step (b), the Li4Ti5O 12 The molar ratio of the lithium source is 0.5-1.5:2-4.

5. The method for preparing Li2TiO3 according to claim 1, characterized in that: The first stirring speed is 120-200 rpm / min.

6. The method for preparing Li2TiO3 according to claim 1, characterized in that: The first stirring time is 2 to 8 hours.

7. The method for preparing Li2TiO3 according to claim 1, characterized in that: The second stirring speed is 150-250 rpm / min.

8. The method for preparing Li2TiO3 according to claim 1, characterized in that: The second stirring time is 1 to 2 hours.

9. The method for preparing Li2TiO3 according to claim 1, characterized in that: The drying temperature is 110-180°C.

10. The method for preparing Li2TiO3 according to claim 1, characterized in that: The second mixed system is dried and crushed to a particle size of less than 150 μm.

11. The method for preparing Li2TiO3 according to claim 1, characterized in that: The first calcination time is 6 to 10 hours.

12. The method for preparing Li2TiO3 according to claim 1, characterized in that: The heating rate of the first calcination is 5-20°C / min.

13. The method for preparing Li2TiO3 according to claim 1, characterized in that: The second calcination time is 4 to 8 hours.

14. The method for preparing Li2TiO3 according to claim 1, characterized in that: The heating rate of the second calcination is 10-20°C / min.

15. The method for preparing Li2TiO3 according to claim 1, characterized in that: The acid solution includes at least one of citric acid, acetic acid or oxalic acid.

16. The method for preparing Li2TiO3 according to claim 1, characterized in that: The lithium source includes at least one of lithium carbonate, lithium hydroxide or lithium chloride.

17. The method for preparing Li2TiO3 according to claim 1, characterized in that: The titanium source includes: titanium dioxide and / or metatitanic acid.

18. A method for preparing a lithium extraction adsorbent, characterized in that: The following steps are involved: The Li2TiO3 prepared by the Li2TiO3 preparation method according to any one of claims 1 to 17 is acidified.

Citation Information

Patent Citations

  • Li2TiO3 powder material, preparation method of Li2TiO3 powder material, and method for preparing spinel lithium titanate with Li2TiO3 powder material

    CN104752708A

  • Synthesis method of lithium extraction adsorbent

    CN110975795A

Cited By

  • A high-temperature lithium extraction adsorbent, its preparation method and application

    CN119549108B