Preparation method and application of high-performance, water-soluble and controllable biomass-based thermoplastic film

High-performance biomass-based thermoplastic films are prepared by composite materials of wine leece protein powder and water-soluble polymers and starch, combined with plasticizers and other regulators, which solves the problem that existing biodegradable plastics are difficult to degrade rapidly in the natural environment. The problem is that efficient and environmentally friendly biodegradable and low-energy production is achieved, and is suitable for the field of degradable packaging.

CN116410606BActive Publication Date: 2024-11-19XIAMEN MITRO NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310276113.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-11-19
Estimated Expiration
2043-03-21

AI Technical Summary

Technical Problem

Existing biodegradable plastic materials are difficult to degrade rapidly in the natural environment, and the production process consumes high energy, making it impossible to achieve a true full life cycle environmental protection cycle and cannot replace disposable petroleum-based plastics.

Method used

Thermoplastic extrusion and film blowing process are carried out using wine lee protein powder, water-soluble polymer and starch composite materials, and the thermoplastic extrusion and film blowing are prepared by adjusting plasticizers, fiber reinforcers, denaturants, reducing agents, dynamic crosslinkers and hydrophobic agents. High-performance, water-soluble controllable biomass-based thermoplastic film.

Benefits of technology

It has achieved excellent strength and ductility of biomass-based thermoplastic films, can quickly degrade under natural conditions, reduce industrial carbon footprint, and is suitable for the field of degradable packaging and reduce industrial composting treatment needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116410606B_ABST
    Figure CN116410606B_ABST
Patent Text Reader

Abstract

The present invention discloses a water-soluble controllable biomass-based thermoplastic film and a preparation method and application thereof, wherein the thermoplastic film is compounded with vinasse protein powder, water-soluble polymer and starch, and is adjusted by a combination of plasticizer, fiber reinforcement, denaturant, reducing agent, dynamic cross-linking agent and hydrophobic agent, and is obtained after thermoplastic extrusion and film blowing. The present invention uses biomass substrate as raw material, and realizes the industrial preparation of biomass-based films with high strength and ductility, controllable water solubility, and natural biodegradability by screw extrusion processing, seamlessly connects the existing polymer plastic processing industry line, has stronger industrial operability, greatly reduces production energy consumption, and has lower industrial carbon emissions. Biomass-based thermoplastic films can be applied to water-soluble packaging, paper-based film packaging, environmentally friendly shopping bags, food packaging and other biodegradable packaging fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoplastic film processing, and in particular relates to a preparation method and application of a high-performance, water-soluble and controllable biomass-based thermoplastic film. Background Art

[0002] White pollution Plastic waste has always been an environmental problem that has plagued the world. According to statistics, about 8 million tons of plastic enter the ocean every year. This means that on average, there are about 15 new plastic bags for every 1 meter of coastline in the world, and it will take more than 400 years for these plastics to completely decompose in the natural environment. If the current trend continues, it is expected that the amount of plastic in the ocean will exceed that of fish by 2050. The shocking plastic waste pollution has caused serious damage to the marine ecology and the earth's environment.

[0003] In order to solve the problem of "white pollution", fully biodegradable plastics and products came into being. Fully biodegradable materials (abbreviated as fully degradable materials), as the name suggests, can be completely decomposed into low molecular compounds (such as CO2 and H2O) by microorganisms (such as bacteria, fungi and algae, etc.) under appropriate and time-limited natural environmental conditions or composting conditions, and will not cause any secondary pollution and pressure to the ecological environment. They are ideal materials to replace disposable plastic products and an important way to solve plastic waste pollution.

[0004] At present, the fully degradable products (shopping bags, garbage bags, ground films, tableware, lunch boxes, straws, etc.) that are widely used in the market are basically based on polylactic acid (PLA), dibasic acid diol copolyester series (PBAT, PBS, PBSA, etc.), starch-based series, cellulose series and their composite materials. Among them, PBAT and PLA are the two most widely used types of biodegradable resin materials. Although PLA and PBAT have good performance and biodegradability, they still have the following shortcomings: Although PLA is derived from bio-based, that is, lactic acid, a product of starch fermentation, it has hidden dangers such as competing with people for food, and PLA is prepared through a small molecule polymerization process to achieve the final product. The polymerization process consumes huge energy, resulting in high costs. PBAT, on the other hand, is derived from petroleum-based raw materials, which is unsustainable from the source of raw materials, and will fluctuate with the price of petroleum raw materials to a certain extent. Degradable products based on PLA and PBAT are basically compostable plastics, which need to be degraded under industrial composting conditions and cannot be degraded quickly under natural conditions. At present, my country's degradable materials are in the initial stage, and back-end processing facilities such as composting plants are not popular. The treatment methods are still mainly landfill and incineration, and effective recycling has not been achieved.

[0005] Biomass film materials have the advantages of renewable raw materials, good biocompatibility, and can be completely degraded in the natural environment after being discarded. They are a perfect substitute for disposable petroleum-based plastics. The earliest and most studied biomass film materials are cellulose film materials, but the single cellulose film material has insufficient mechanical properties and poor film ductility. It cannot be efficiently industrialized through the existing polymer thermoplastic processing system. It can only be obtained by dissolving in a specific solvent and then using steel strip casting to obtain film products. The processing occupies a large area, the drying process consumes a lot of energy, and there are problems such as complex solvent system recovery. In order to solve the above problems, the technical solution of the patent number 2021116098438 previously applied by the applicant realizes the industrial preparation of water-soluble films of fully degradable thermoplastics made of bio-based distiller's grains protein, but it has a narrow range of applications and is only used in the field of water-soluble films. At the same time, its strength and ductility properties are still lacking.

[0006] It is particularly important to realize the source and use of raw materials, truly achieve the reasonable consumption of green resources, produce pollution-free products that are friendly to the environment and humans in the manufacturing process, and recycle and reuse and dispose of waste in the final link, so as to truly return to nature for a virtuous cycle, realize a true full life cycle system, and effectively solve the problem of white pollution.

[0007] Based on this, we proposed a method for preparing a bio-based thermoplastic film that has excellent strength and ductility, controllable water solubility, large-scale industrial thermoplastic processing, and good biodegradability, and conducted commercial exploration of its application in the field of degradable packaging. Summary of the invention

[0008] In view of the above-mentioned technical problems, the purpose of the present invention is to design and provide a technical solution for the preparation method and application of a high-performance, water-soluble and controllable biomass-based thermoplastic film.

[0009] The present invention is achieved through the following technical solutions:

[0010] The present invention provides a high-performance, water-soluble and controllable biomass-based thermoplastic film, which is compounded by distiller's grains protein micropowder, water-soluble polymer and starch, and adjusted by plasticizer, fiber reinforcement agent, denaturant, reducing agent, dynamic cross-linking agent and hydrophobic agent, and then obtained by thermoplastic extrusion and film blowing processing.

[0011] Furthermore, the thermoplastic film comprises the following components in parts by weight: 10-80 parts of wine lees protein powder, 10-80 parts of starch, 2-30 parts of water-soluble polymer, 2-50 parts of environmentally friendly plasticizer, 1-10 parts of fiber reinforcement, 1-2 parts of reducing agent, 1-2 parts of dynamic cross-linking agent, 1-2 parts of hydrophobic agent, and 1-2 parts of denaturant.

[0012] Furthermore, the wine lees protein powder is obtained by grafting and spray drying the wine lees protein separated and purified from wine lees waste, wherein the modification is any one of epoxy modification and acylation modification.

[0013] Furthermore, the starch is at least one of high-amylose starch, oxidized high-amylose starch, and carboxymethyl high-amylose starch, wherein the amylose content is ≥50%.

[0014] Furthermore, the water-soluble polymer is any one of polyvinyl alcohol, sodium alginate and polyvinyl pyrrolidone.

[0015] Furthermore, the plasticizer is at least one of pure water, glycerol, sorbitol, polyglycerol, polyglycerol fatty acid monoester, and formamide; the fiber reinforcement is at least one of cellulose nanofibers, cationized cellulose nanofibers, and carboxymethylated cellulose nanofibers, preferably with an aspect ratio ≥500, and more preferably with an aspect ratio ≥1000; the denaturant is any one of guanidine hydrochloride, urea, and SDS; the reducing agent is any one of 2-mercaptoethanol, sodium sulfite, and dithiothreitol; the dynamic cross-linking agent is at least one of calcium oxide, calcium chloride, and alum; and the hydrophobic agent is any one of oleamide and erucamide.

[0016] The second object of the present invention is to provide a method for preparing a high-performance, water-soluble and controllable biomass-based thermoplastic film, comprising the following steps:

[0017] 1) stirring and mixing the vinasse protein powder, water-soluble polymer, starch, fiber reinforcing agent, denaturing agent, reducing agent, dynamic cross-linking agent and hydrophobic agent according to the formula amount to obtain a premix;

[0018] 2) placing the plasticizer in the formula amount and the premix obtained in step 1) in a twin-screw extruder at 90-135° C. for thermoplastic processing by means of side-pumping metered liquid feeding, cooling and pelletizing to obtain a biomass-based thermoplastic masterbatch;

[0019] 3) The biomass-based thermoplastic masterbatch obtained in step 2) is subjected to single-screw extrusion blown film to obtain a rolled biomass-based thermoplastic film.

[0020] The third object of the present invention is to provide the use of biomass-based thermoplastic film in degradable packaging materials.

[0021] Furthermore, the degradable packaging materials are specifically used in the field of biodegradable packaging such as water-soluble packaging, paper-based film packaging, environmentally friendly shopping bags, and food packaging.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1) Biomass-based thermoplastic film has excellent strength and ductility (when the biomass content exceeds 80%, the maximum tensile strength can reach 25MPa and the elongation at break is 98%), oxygen barrier performance (≤2cm 3 / (m 2 ·24h)), heat-sealing packaging performance, can adapt to the existing polymer plastic processing system, and more importantly, it is derived from biomass, can be naturally degraded, does not require industrial composting, has lower carbon dioxide emissions, is more environmentally friendly, and can be widely used in water-soluble packaging, paper-based film packaging, environmentally friendly shopping bags, food packaging and other biodegradable packaging fields;

[0024] 2) Using protein from waste distiller's grains as a biomass substrate to prepare degradable packaging film materials not only achieves efficient utilization of distiller's grains agricultural waste, turning waste into treasure, but also reduces industrial energy consumption without the need for small molecule repolymerization. The final product has excellent biodegradability, can be rapidly degraded in the natural environment, and has a lower industrial carbon footprint;

[0025] 3) In the vinasse protein matrix, high-amylose starch rigid molecular chains and high-molecular-weight water-soluble polymer flexible molecular chains are introduced to achieve network interpenetration among the three, and the hydrogen bonds between the three are used to form an interwoven three-dimensional network structure, which has higher strength and toughness than a single biomass-based film;

[0026] 4) The fiber skeleton network of cellulose nanofibers with high aspect ratio and high specific surface area is used to form a steel-concrete structure. At the same time, the hydrogen bonding between the protein matrix and the cellulose nanofibers further effectively improves the strength of the bio-based film, and further intersperses metal ions for dynamic cross-linking. Compared with chemical disordered cross-linking, metal ion cross-linking has better thermoplastic processability and dynamic toughness;

[0027] 5) The preparation of biomass-based thermoplastic film with controllable water solubility was achieved by modifying distiller's grains protein, selecting starch and water-soluble polymer types, and optimizing the formulation;

[0028] 6) It realizes the thermoplastic processing of biomass-based materials, which is perfectly adapted to the existing polymer thermoplastic processing system. It does not require conventional tape-casting steel belts and drying units, greatly reduces drying energy consumption, and effectively improves production and processing efficiency and production output. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The biomass-based thermoplastic resin masterbatch prepared in Example 1 of the present invention;

[0030] Figure 2 The biomass-based rolled thermoplastic film prepared in Example 1 of the present invention;

[0031] Figure 3This is a sample of laundry detergent packaging based on biomass-based thermoplastic film. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with specific embodiments to facilitate a better understanding of the present technical solution.

[0033] The test and characterization methods for the bio-based film strength, water solubility, oxygen permeability, water absorption and contact angle in the following examples are as follows:

[0034] 1. After the film samples were placed in a constant temperature and humidity chamber (23°C, 50RH%) for 24 hours, the film strength was measured according to ISO1184-1983 "Determination of tensile properties of plastic films".

[0035] 2. Cut the biomass-based film into 6×6 cm squares (thickness between 50-75 μm), immerse it in a glass watch glass filled with room temperature water, keep it static and without stirring, and observe the time it takes for the film to completely dissolve to judge the water solubility of the film.

[0036] 3. Use MOCON The 2 / 22 gas permeometer (U.S. Membrane Con) was used to measure the oxygen permeability of biomass-based thermoplastic films according to GB / T1038-2000.

[0037] Example 1

[0038] The preparation process of the biomass-based thermoplastic film in this embodiment is as follows:

[0039] (1) Epoxy modification of distillers grains protein

[0040] The vinasse protein separated and purified from vinasse waste is placed in a stainless steel reactor and diluted with water to a suspension with a solid content of about 20-25wt%. Subsequently, a 0.5mol / L sodium hydroxide solution is used to adjust the pH of the entire suspension system to about 9, and the heating temperature is controlled to 80°C. Finally, 15% of tert-butyl glycidyl ether relative to the absolute dry mass of the vinasse protein is added, the stirring speed is set to 200r / min, and the reaction time is 2h to achieve epoxy grafting modification of the vinasse protein.

[0041] After the reaction is completed, the pH of the wine lees protein suspension is adjusted to neutral, and the solid content is adjusted to between 8% and 10% by weight. After spray drying, the modified wine lees protein powder is obtained for subsequent thermoplastic processing.

[0042] (2) Thermoplastic extrusion processing and film blowing

[0043] a. Place modified distiller's grain protein powder, high amylose starch (amylose content 55%), polyvinyl alcohol particles (polymerization degree of about 1700, alcoholysis degree 88%), and hydrophobic agent (oleic acid amide) in a high-speed mixer for high-speed blending, set the speed to 300r / min, and evenly mix for 15 minutes to obtain a fully mixed premix. The proportions of the components of the premix are, by weight, 60 parts of modified distiller's grain protein powder, 20 parts of high amylose starch, 20 parts of polyvinyl alcohol, and 2 parts of oleic acid amide.

[0044] b. Dissolve the fiber reinforcing agent (cellulose nanofiber, aspect ratio ≥ 1000), reducing agent (sodium sulfite), denaturing agent (urea), and dynamic crosslinking agent (calcium oxide) in pure water, then add other non-aqueous plasticizers and mix thoroughly to prepare a liquid mixture. The proportion of each component, by weight, is 15 parts of pure water, 25 parts of glycerol, 3 parts of cellulose nanofiber, 1 part of sodium sulfite, 1 part of urea, and 1 part of calcium oxide.

[0045] c. The obtained uniformly mixed powder material is transferred to a twin-screw extruder, and pumping and metering are used to achieve uniform feeding of the liquid mixture from the side. The screw diameter is 25dm, the aspect ratio is 40, and the temperatures of each zone in each heating section are set to 60℃, 80℃, 100℃, 105℃, 105℃, 105℃, 105℃, 100℃, respectively. The head temperature is 100℃, the main screw speed is 80r / min, and the feeding speed is 30r / min. After twin-screw extrusion, drawing, cooling, and pelletizing, biomass-based thermoplastic masterbatch is obtained, as shown in the picture Figure 1 shown.

[0046] d. The biomass-based thermoplastic masterbatch obtained by extrusion pelletization is processed by single screw extrusion film blowing to achieve the preparation of biomass-based thermoplastic film. The screw extrusion film blowing processing temperature range is set to 80°C, 100°C, 110°C, 110°C, and 105°C. The obtained biomass-based rolled thermoplastic film is as follows: Figure 2 shown.

[0047] The strength of the biomass-based film is 16.75±1.65MPa, the elongation at break is 145.68±12.57%, and the static water dissolution time is about 8min.

[0048] Example 2

[0049] The difference from Example 1 is that the amount of cellulose nanofiber reinforcing agent used is 1 part.

[0050] Example 3

[0051] The difference from Example 1 is that the amount of cellulose nanofiber reinforcing agent used is 5 parts.

[0052] Example 4

[0053] The difference from Example 1 is that the cellulose reinforcing agent is cationized cellulose nanofibers, and the cationic charge density is 0.36 mmol / g.

[0054] Example 5

[0055] The difference from Example 1 is that the high-amylose starch is 10 parts and the polyvinyl alcohol is 30 parts;

[0056] Example 6

[0057] The difference from Example 1 is that the high-amylose starch is 30 parts and the polyvinyl alcohol is 10 parts;

[0058] Comparative Example 1

[0059] The difference from Example 1 is that no fiber reinforcement is added.

[0060] The experimental formulas and film performance data of Example 1 and Comparative Examples 1-6 are shown in Table 1.

[0061] Table 1

[0062]

[0063] Example 7

[0064] The difference from Example 1 is that the dynamic cross-linking agent is alum, 1 part by weight.

[0065] The strength of the bio-based film is 16.87±0.58MPa, the elongation at break is 110.78±13.91%, and the static water dissolution time is 9min.

[0066] Example 8

[0067] The difference from Example 1 is that the modification of vinasse protein is carried out according to the following steps:

[0068] The lees protein separated and purified from the lees waste is placed in a stainless steel reactor and diluted with water to a suspension with a solid content of about 20-25wt%. Subsequently, a 0.5mol / L sodium hydroxide solution is used to adjust the pH of the entire suspension system to 11, and the heating temperature is controlled to 100°C. Finally, 30% of epichlorohydrin relative to the absolute dry mass of the lees protein is added, the stirring speed is set to 200r / min, and the reaction time is 4h to achieve epoxy grafting modification of the lees protein.

[0069] After the reaction is completed, the pH of the wine lees protein suspension is adjusted to neutral, and the solid content is adjusted to between 8% and 10% by weight. After spray drying, the modified wine lees protein powder is obtained for subsequent thermoplastic processing.

[0070] The polyvinyl alcohol model was adjusted to a degree of polymerization of about 2400 and a degree of alcoholysis of 88%.

[0071] The strength of the bio-based film is 18.31±1.58MPa, the elongation at break is 217.19±16.24%, and the static water dissolution time is 5min.

[0072] Example 9

[0073] The difference from Example 8 is that the starch used is carboxymethylated high-amylose starch, the degree of substitution is 0.58, and the amylose content is 55%.

[0074] The strength of the bio-based film is 18.44±1.19MPa, the elongation at break is 225.98±10.72%, and the static water dissolution time is 3min.

[0075] Example 10

[0076] The difference from Example 1 is that the amylose content in the high amylose starch is increased to 70%, the polyvinyl alcohol type is adjusted to a polymerization degree of about 2200, and the alcoholysis degree is 99%. The plasticizer formula is adjusted to 25 parts of pure water, 20 parts of glycerol, and 5 parts of decaglycerol.

[0077] The screw extrusion processing temperature was set to 80℃, 90℃, 100℃, 110℃, 110℃, 110℃, 105℃, 105℃, and the film blowing temperature was set to 80℃, 100℃, 115℃, 120℃, 120℃, 115℃.

[0078] The bio-based film has a strength of 19.57±1.29MPa, an elongation at break of 167.13±21.74%, is insoluble in water under static conditions, and an oxygen permeability test result of 1.97±0.15cm 3 / (m 2 ·24h).

[0079] Embodiment 11

[0080] The difference from Example 10 is that the modification of vinasse protein is carried out according to the following steps:

[0081] The lees protein separated and purified from the lees waste is placed in a stainless steel reactor and diluted with water to a suspension with a solid content of about 20-25wt%. Subsequently, 5 times the absolute dry mass of the lees protein, 2 times the acetic anhydride, and 5% concentrated sulfuric acid are added, and the mixture is stirred continuously. The acylation reaction temperature is 75°C and the reaction time is 3h to achieve acetylation modification of the lees protein.

[0082] After the reaction is completed, the distiller's grains protein suspension is washed to neutrality, and the solid content is adjusted to between 8% and 10% by weight. After spray drying, the modified distiller's grains protein powder is obtained for subsequent thermoplastic processing.

[0083] The bio-based film has a strength of 20.61±1.41MPa, an elongation at break of 150.12±14.28%, is insoluble in water under static conditions, and the oxygen permeability is 1.56±0.32cm 3 / (m 2 ·24h).

[0084] Comparative Example 2: Prior application of the applicant, application number is 2021116098438

[0085] The fully degradable thermoplastic water-soluble film in this comparative example is prepared as follows:

[0086] (1) Modification of distillers grains protein

[0087] The lees protein precipitate after protein extraction, separation and purification is placed in a stainless steel reactor and diluted with water to a suspension with a solid content of about 20-25wt%. Subsequently, the pH of the entire suspension system is adjusted to about 10 using a 0.5mol / L sodium hydroxide solution, and the heating temperature is controlled to 90°C. Finally, 25%wt of an epoxy grafting agent, specifically propylene oxide, is added relative to the absolute dry mass of the lees protein. The stirring speed is set to 200r / min and the reaction time is 2h, thereby simultaneously achieving the salting regulation and epoxy grafting modification of the lees protein.

[0088] After the reaction is completed, the pH of the wine lees protein suspension is adjusted to neutral, and the solid content is adjusted to between 8-10%wt. After spray drying, the modified wine lees protein powder is obtained for subsequent thermoplastic processing.

[0089] (2) Thermoplastic extrusion processing and film blowing

[0090] a. Dissolve the reducing agent sodium sulfite and the co-solvent polyether polyol in pure water, then add glycerol and mix thoroughly, pour into the propylene oxide modified vinasse protein powder, place in a high-speed mixer for high-speed blending, set the speed to 300r / min, and mix evenly for 15 minutes to obtain a fully mixed premix. The proportions of the components of the premix, by weight, are 75 parts of modified vinasse protein powder, 10 parts of pure water, 15 parts of glycerol, 1 part of sodium sulfite, 1 part of polyether polyol, 2 parts of oleic acid, and 1 part of calcium chloride.

[0091] b. The obtained mixed material is transferred to a twin-screw extruder with a screw diameter of 25 dm and an aspect ratio of 40. The temperatures of each zone in each heating section are set to 40°C, 60°C, 80°C, 100°C, 100°C, 90°C, and 90°C, respectively. The head temperature is 90°C, the main screw speed is 100 r / min, and the feeding speed is 30 r / min. After twin-screw extrusion, drawing, cooling, and pelletizing, the wine grains protein film masterbatch is obtained.

[0092] c. The vinasse film masterbatch obtained by extrusion pelletization was placed in a constant temperature and humidity environment (23°C, 50% RH) for 24 hours for equilibrium treatment, and then single-screw extrusion film blowing was used to prepare the vinasse protein thermoplastic water-soluble. The screw extrusion film blowing processing temperature range was set to 80°C, 100°C, 110°C, 110°C, and 100°C.

[0093] The strength of the biomass-based film is 13.91±0.52MPa, the elongation at break is 135±8%, and the static water dissolution time is 5min.

[0094] Comparative Example 3

[0095] The difference from Example 1 is that no modified distiller's grains protein powder is added, and the amount of high-amylose starch is 90 parts and the amount of polyvinyl alcohol is 10 parts.

[0096] The strength of the biomass-based film is 10.28±0.47MPa, the elongation at break is 66.28±12.23%, and it is insoluble in water under static conditions. Due to the crystalline structure of starch and the regeneration phenomenon, some films of this comparative example are prone to packaging breakage after being placed for a period of time.

[0097] The present invention uses protein from waste wine lees as a biomass substrate to prepare a degradable packaging film material, and achieves the preparation of a biomass-based thermoplastic film with high strength, high ductility, and controllable water solubility through structural and formula regulation. The biomass-based thermoplastic film has excellent strength properties, ductility properties, packaging properties, and oxygen barrier properties, and is biodegradable under natural conditions without the need for industrial composting. The biomass-based thermoplastic film in Example 4 has a biomass content of up to 80%, excellent strength properties, and good water solubility. It can replace the existing petroleum-based polyvinyl alcohol water-soluble film and can be used in the field of water-soluble films. The biomass thermoplastic film in Example 11 has a strength property of more than 20MPa, and has good ductility, and an oxygen barrier property of less than 2cm. 3 / (m 2 ·24h), which is comparable to existing PVDC barrier materials and can be used for fresh-keeping barrier packaging of high-fat and high-protein foods. According to different application performance requirements, the biomass-based thermoplastic water-soluble film prepared by the present invention can be widely used in water-soluble packaging (laundry beads, dishwashing beads, pesticide packaging, etc.), such as the packaging of laundry beads. Figure 3 As shown in the following biodegradable packaging fields: paper-based composite packaging, environmentally friendly shopping bags, food packaging, etc.

Claims

1. A high-performance, water-soluble, controllable biomass-based thermoplastic film, characterized in that: The thermoplastic film is compounded by distiller's grains protein powder, water-soluble polymer and starch, and adjusted by plasticizer, fiber reinforcing agent, denaturant, reducing agent, dynamic cross-linking agent and hydrophobic agent, and then obtained by thermoplastic extrusion and film blowing. The thermoplastic film comprises the following components in parts by weight: 10-80 parts of wine lees protein powder, 10-80 parts of starch, 2-30 parts of water-soluble polymer, 2-50 parts of environmentally friendly plasticizer, 1-10 parts of fiber reinforcing agent, 1-2 parts of reducing agent, 1-2 parts of dynamic cross-linking agent, 1-2 parts of hydrophobic agent, and 1-2 parts of denaturant; The starch is at least one of high-amylose starch and carboxymethyl high-amylose starch, wherein the amylose content is ≥50%; the water-soluble polymer is polyvinyl alcohol; and the fiber reinforcing agent is at least one of cellulose nanofibers and cationic cellulose nanofibers.

2. A high-performance, water-soluble, controllable biomass-based thermoplastic film as claimed in claim 1, characterized in that: The vinasse protein powder is obtained by grafting and modifying vinasse protein separated and purified from wine tank waste and spray drying, wherein the modification is any one of epoxy modification and acylation modification.

3. A high-performance, water-soluble, controllable biomass-based thermoplastic film as claimed in claim 1, characterized in that: The plasticizer is at least one of pure water, glycerol, sorbitol, polyglycerol, polyglycerol fatty acid monoester, and formamide; The denaturant is any one of guanidine hydrochloride, urea, and SDS; The reducing agent is any one of 2-mercaptoethanol, sodium sulfite, and dithiothreitol; The dynamic cross-linking agent is at least one of calcium oxide, calcium chloride and alum; The hydrophobic agent is any one of oleamide and erucamide.

4. A method for preparing a high-performance, water-soluble, controllable biomass-based thermoplastic film according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: 1) stirring and mixing the wine lees protein powder, water-soluble polymer, starch, fiber reinforcing agent, denaturing agent, reducing agent, dynamic cross-linking agent and hydrophobic agent according to the formula amount to obtain a premix; 2) The plasticizer in the formula and the premix obtained in step 1) are placed in a twin-screw extruder at 90-135° C. for thermoplastic processing by means of side-pumping metered liquid feeding, and after cooling and pelletizing, a biomass-based thermoplastic masterbatch is obtained; 3) The biomass-based thermoplastic masterbatch obtained in step 2) is subjected to single-screw extrusion film blowing to obtain a rolled biomass-based thermoplastic film.

5. Use of the high-performance, water-soluble, controllable biomass-based thermoplastic film as claimed in any one of claims 1 to 3 in degradable packaging materials.