A foam metal supported nickel ferrite monolithic catalyst and its preparation method and application

By using foam metal-supported nickel ferrite catalysts in methane catalytic cracking, the problems of low activity and ease of inactivation in traditional catalysts are solved, and efficient methane catalytic and stable catalytic properties are achieved.

CN116422334BActive Publication Date: 2024-11-22INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310290084.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2023-03-23
Publication Date
2024-11-22
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Traditional catalysts are low in activity and are prone to inactivation in methane catalytic cracking, making it difficult to meet the needs of efficient hydrogen production reactions.

Method used

The foam metal-supported nickel ferrite monolithic catalyst was prepared by in-situ electrodeposition method, using the anti-spinel structure of nickel ferrite and the high specific surface area and pore structure of foam metal, combining the presence of nickel salt and iron salt , improve the activity and stability of the catalyst.

Benefits of technology

High methane catalytic activity and stability are achieved, the preparation process is simplified, raw material waste is reduced, and the long-term use effect of the catalyst is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004141101680000121
    Figure BDA0004141101680000121
  • Figure BDA0004141101680000131
    Figure BDA0004141101680000131
Patent Text Reader

Abstract

The present invention provides a foam metal-supported nickel ferrite monolithic catalyst and a preparation method and application thereof. The preparation method is as follows: (1) using metal foam as a cathode and a first solution as an electrodeposition liquid to perform electrodeposition to obtain a monolithic catalyst precursor; (2) cleaning the monolithic catalyst precursor obtained in step (1), and calcining to obtain the foam metal-supported nickel ferrite monolithic catalyst; the first solution in step (1) contains nickel salt and iron salt. The foam metal-supported nickel ferrite monolithic catalyst provided by the present invention has high activity and stability, and solves the problems of low activity and easy deactivation of traditional catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of methane cracking catalyst preparation, and relates to an integral catalyst, in particular to a foam metal-supported nickel ferrite integral catalyst and a preparation method and application thereof. Background Art

[0002] With the continuous increase in proven reserves of natural gas resources, methane has contributed 20% to the global temperature rise caused by anthropogenic greenhouse gas emissions, and has become the second largest greenhouse gas component after CO2. Hydrogen, as an environmentally friendly fuel with high energy density, high combustion calorific value and no pollution, is an important energy carrier in sustainable development. Among the many methods of hydrogen production, the catalytic cracking of methane to produce hydrogen does not produce CO or CO2, and pure hydrogen can be obtained.

[0003] Nickel ferrite has an inverse spinel structure. Nickel ions occupy the octahedral sites of the unit cell, and iron ions occupy the tetrahedral sites and half of the octahedral sites of the unit cell. Because nickel ions occupy the octahedral sites, they exhibit a mixed state of trivalent and divalent ions. This unstable structure often has abundant crystal defects, which makes nickel ferrite exhibit excellent catalytic properties.

[0004] Foam metals have the characteristics of low density, high specific surface area, and rich pore structure, and are widely used as catalyst carrier materials. Ionic liquids are organic salts composed of anions and cations, which are liquid at room temperature and have good conductivity, good stability, and a wide electrochemical window.

[0005] Electrodeposition is a new material preparation method. Under the action of an external electric field, the ions in the solution undergo redox reactions and are directly deposited on the electrode material in the form of metals, alloys or oxides. During the experiment, the morphology and composition of the deposited layer can be controlled by changing the electrodeposition process parameters. It is a fast, simple and low-cost method for preparing monolithic catalysts. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a foam metal supported nickel ferrite monolithic catalyst and its preparation method and application. The foam metal supported nickel ferrite monolithic catalyst has high catalytic activity and stability, solving the problems of low activity and easy deactivation of traditional catalysts.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a foam metal supported nickel ferrite monolithic catalyst, the preparation method being as follows:

[0009] (1) using metal foam as a cathode and a first solution as an electrodeposition solution to perform electrodeposition to obtain a monolithic catalyst precursor;

[0010] (2) cleaning the monolithic catalyst precursor obtained in step (1), and calcining the monolithic catalyst to obtain the foam metal-supported nickel ferrite monolithic catalyst;

[0011] Step (1) The first solution contains nickel salt and iron salt.

[0012] The present invention adopts an in-situ electrodeposition method to prepare the foam metal-loaded nickel ferrite monolithic catalyst, and its preparation principle is: when power is turned on, nitrate ions near the cathode are reduced to generate a large number of hydroxide ions, and then the metal ions in the solution react with the hydroxide ions on the cathode surface to generate hydroxides that precipitate on the cathode surface.

[0013] The active components in the foam metal-loaded nickel ferrite monolithic catalyst obtained by the preparation method provided by the present invention include nickel salt and iron salt. The presence of the nickel salt improves the catalytic activity of the catalyst, and the presence of the iron salt improves the stability of the catalyst, thereby solving the problem of low activity and easy deactivation of traditional catalysts.

[0014] As a preferred technical solution of the present invention, the metal foam in step (1) includes any one of nickel foam, aluminum foam or copper foam.

[0015] Preferably, the pore size of the metal foam in step (1) is 50 to 500 μm, for example, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm or 500 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] Preferably, the preparation method further comprises a pretreatment process of the metal foam in step (1).

[0017] Preferably, the pretreatment process is to sequentially clean the metal foam with hydrochloric acid, anhydrous ethanol, acetone and deionized water.

[0018] Preferably, the hydrochloric acid cleaning time is 20 to 50 s, for example, it can be 20 s, 24 s, 28 s, 32 s, 36 s, 40 s, 44 s, 48 ​​s or 50 s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the concentration of hydrochloric acid in the hydrochloric acid cleaning is 1.5-2.5 mol / L, for example, it can be 1.5 mol / L, 1.7 mol / L, 1.9 mol / L, 2.1 mol / L, 2.3 mol / L or 2.5 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the water-ethanol cleaning time is 8 to 15 minutes, for example, it can be 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the acetone cleaning time is 8 to 15 minutes, for example, it can be 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] The pretreatment process of the present invention is used to remove oxides and stains on the surface of metal foam and promote surface roughening.

[0023] Preferably, the preparation method of the electrodeposition solution in step (1) is: mixing an active component solution and an ionic liquid, and stirring and mixing them uniformly to obtain the electrodeposition solution.

[0024] Preferably, the mass ratio of the active component solution to the ionic liquid is 1:(1.5-3.5), for example, 1:1.5, 1:1.9, 1:2.3, 1:2.7, 1:3.1 or 1:3.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the ionic liquid includes any one of 1-ethyl-3-methylimidazole, 1-butyl-3-methylimidazole chloride, 1-hexadecyl-3-methylimidazole chloride, 1-ethyl-3-methylimidazole tetrafluoroborate, 1-butyl-3-methylimidazole tetrafluoroborate, 1-ethyl-3-methylimidazole bis-trifluoromethanesulfonyl imide salt, 1-butyl-3-methylimidazole bis-trifluoromethanesulfonyl imide salt or 1-butyl-3-methylimidazole hexafluoroborate or a combination of at least two thereof, and a typical but non-limiting combination includes 1-ethyl-3-methyl imidazole, a combination of 1-butyl-3-methylimidazole chloride and 1-hexadecyl-3-methylimidazole chloride, a combination of 1-ethyl-3-methylimidazole tetrafluoroborate and 1-butyl-3-methylimidazole tetrafluoroborate, a combination of 1-ethyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt and 1-butyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt, or a combination of 1-ethyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt, 1-butyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt and 1-butyl-3-methylimidazole hexafluoroborate.

[0026] The ionic liquid in the electrodeposition solution of the present invention can form a coordination relationship with the metal ions, so that the metal ions can grow in situ on the surface of the nickel foam.

[0027] Preferably, the active component solution is a mixed solution of nickel salt and iron salt.

[0028] Preferably, the nickel salt comprises nickel nitrate.

[0029] Preferably, the iron salt comprises ferric nitrate.

[0030] Preferably, the concentration ratio of nickel salt to iron salt in the active component solution is 1:(0.1-0.4), for example, it can be 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35 or 1:0.4, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the deposition potential of the electrodeposition in step (1) is -0.5 to -1.5 V, for example, -0.5 V, -0.7 V, -0.9 V, -1.1 V, -1.3 V or -1.5 V, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the deposition time of the electrodeposition in step (1) is 1 to 3 minutes, for example, 1 minute, 1.4 minutes, 1.8 minutes, 2.2 minutes, 2.6 minutes or 3 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the electrodeposition temperature in step (1) is 20-60°C, for example, 20°C, 30°C, 40°C, 50°C or 60°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] The deposition potential in the electrodeposition process of the present invention is limited to -0.5 to -1.5 V. If the deposition potential is too high, the load thickness will increase, the precipitation layer will stack, and the final catalytic performance will be reduced; if the deposition potential is too low, the amount of precipitate generated will be reduced, and a high-activity catalyst cannot be obtained.

[0035] Preferably, the counter electrode in the electrodeposition in step (1) is a platinum sheet, and the reference electrode is a saturated calomel electrode.

[0036] Preferably, the cleaning in step (2) comprises rinsing the monolithic catalyst precursor with deionized water;

[0037] Preferably, the calcination temperature in step (2) is 500-800°C, for example, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] The calcination temperature of the present invention is 500-800° C. If the temperature is too high, the nickel ferrite will be melted and sintered, reducing the effective components of the catalyst; if the temperature is too low, the precursor cannot be completely converted and good catalytic activity cannot be obtained.

[0039] Preferably, the calcination time in step (2) is 3 to 5 h, for example, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h, 4 h, 4.2 h, 4.4 h, 4.6 h, 4.8 h or 5 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] As a preferred technical solution of the present invention, the preparation method of the foam metal supported nickel ferrite monolithic catalyst provided in the first aspect of the present invention comprises the following steps:

[0041] (1) using metal foam as a cathode, the first solution as an electrodeposition solution, a platinum sheet as a counter electrode, and a saturated calomel electrode as a reference electrode, and performing electrodeposition for 1 to 3 minutes at a potential of -1.0 to -1.5 V and a temperature of 20 to 40° C. to obtain a monolithic catalyst precursor;

[0042] The metal foam is pretreated, specifically, the metal foam is sequentially washed with hydrochloric acid for 20 to 50 seconds, washed with anhydrous ethanol for 8 to 15 minutes, washed with acetone for 8 to 15 minutes, and washed with deionized water; the concentration of hydrochloric acid in the hydrochloric acid washing is 1.5 to 2.5 mol / L;

[0043] The preparation method of the electrodeposition solution is: mixing the active component solution and the ionic liquid in a mass ratio of 1: (1.5-3.5), stirring and mixing to obtain the electrodeposition solution;

[0044] The active component solution contains iron nitrate and nickel nitrate, and the concentration ratio of nickel nitrate to iron nitrate in the active component solution is 1:(0-0.4);

[0045] (2) The monolithic catalyst precursor obtained in step (1) is washed with deionized water, and calcined at 500-800° C. for 3-5 hours to obtain the foam metal-supported nickel ferrite monolithic catalyst.

[0046] In a second aspect, the present invention provides a foam metal-supported nickel ferrite monolithic catalyst obtained by the method for preparing the foam metal-supported nickel ferrite monolithic catalyst provided in the first aspect.

[0047] In a third aspect, the present invention provides an application of a foam metal-supported nickel ferrite monolithic catalyst prepared by the preparation method provided in the first aspect, wherein the foam metal-supported nickel ferrite monolithic catalyst is used for methane cracking to produce hydrogen.

[0048] Preferably, the methane cracking to produce hydrogen is carried out in a fixed bed reactor.

[0049] Preferably, the temperature in the methane cracking hydrogen production is 500-800°C, for example, 500°C, 600°C, 700°C or 800°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] Preferably, the raw material for producing hydrogen by cracking methane is a CH4 / Ar mixed gas, and the content of methane in the mixed gas is 20%.

[0051] Preferably, the flow rate of the raw material in the methane cracking hydrogen production is 20-30 mL / min, for example, it can be 20 ml / min, 22 ml / min, 24 ml / min, 26 ml / min, 28 ml / min or 30 ml / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The foam metal supported nickel ferrite monolithic catalyst provided by the present invention adopts NiFe2O4 inverse spinel structure rich in intrinsic defects as an active component, and a high specific surface area and porous foam metal as a carrier, and has high methane catalytic activity and stability;

[0055] (2) The present invention adopts an in-situ electrodeposition method to prepare a foam metal-supported nickel ferrite monolithic catalyst, which simplifies the preparation process, reduces the preparation time, and avoids the waste of raw materials. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] Example 1

[0058] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst, and the preparation method of the foam metal supported nickel ferrite monolithic catalyst comprises the following steps:

[0059] (1) using a nickel foam sheet as a cathode, the first solution as an electrodeposition solution, a platinum sheet as a counter electrode, and a saturated calomel electrode as a reference electrode, and performing electrodeposition for 2 min at a potential of -1.0 V and 20° C. to obtain a monolithic catalyst precursor;

[0060] The nickel foam sheet is pretreated, specifically, the nickel foam sheet is sequentially cleaned with hydrochloric acid for 30 seconds, anhydrous ethanol for 10 minutes, acetone for 10 minutes, and deionized water; the concentration of hydrochloric acid in the hydrochloric acid cleaning is 2 mol / L;

[0061] The preparation method of the electrodeposition solution is as follows: mixing the active component solution and 1-hexadecyl-3-methylimidazole chloride in a mass ratio of 1:2, stirring and mixing to obtain the electrodeposition solution;

[0062] The active component solution contains nickel nitrate and ferric nitrate, wherein the concentration of the nickel nitrate is 0.1 mol / L, and the concentration of the ferric nitrate is 0.03 mol / L;

[0063] (2) The monolithic catalyst precursor obtained in step (1) is washed with deionized water, and calcined at 700° C. for 4 hours to obtain the foam metal-supported nickel ferrite monolithic catalyst.

[0064] Example 2

[0065] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst, and the preparation method of the foam metal supported nickel ferrite monolithic catalyst comprises the following steps:

[0066] (1) using an aluminum foam sheet as a cathode, the first solution as an electrodeposition solution, a platinum sheet as a counter electrode, and a saturated calomel electrode as a reference electrode, and performing electrodeposition at a potential of -1.0 V and 30° C. for 1 min to obtain a monolithic catalyst precursor;

[0067] The foam aluminum sheet is pretreated, specifically, the foam aluminum sheet is sequentially cleaned with hydrochloric acid for 20 seconds, anhydrous ethanol for 8 minutes, acetone for 8 minutes, and deionized water; the concentration of hydrochloric acid in the hydrochloric acid cleaning is 2.5 mol / L;

[0068] The preparation method of the electrodeposition solution is as follows: mixing the active component solution and 1-butyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt at a mass ratio of 1:3.5, stirring and mixing evenly to obtain the electrodeposition solution;

[0069] The active component solution contains nickel nitrate and ferric nitrate, wherein the concentration of the nickel nitrate is 0.1 mol / L, and the concentration of the ferric nitrate is 0.04 mol / L;

[0070] (2) The monolithic catalyst precursor obtained in step (1) is washed with deionized water, and calcined at 500° C. for 5 h to obtain the foam metal-supported nickel ferrite monolithic catalyst.

[0071] Example 3

[0072] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst, and the preparation method of the foam metal supported nickel ferrite monolithic catalyst comprises the following steps:

[0073] (1) using a copper foam sheet as a cathode, the first solution as an electrodeposition solution, a platinum sheet as a counter electrode, and a saturated calomel electrode as a reference electrode, and performing electrodeposition at a potential of -1.0 V and 40° C. for 3 min to obtain a monolithic catalyst precursor;

[0074] The copper foam sheet is pretreated, specifically, the copper foam sheet is sequentially cleaned with hydrochloric acid for 50 seconds, anhydrous ethanol for 15 minutes, acetone for 15 minutes, and deionized water; the concentration of hydrochloric acid in the hydrochloric acid cleaning is 2.5 mol / L;

[0075] The preparation method of the electrodeposition solution is as follows: mixing the active component solution and 1-ethyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt at a mass ratio of 1:1.5, stirring and mixing evenly to obtain the electrodeposition solution;

[0076] The active component solution contains nickel nitrate and ferric nitrate, wherein the concentration of the nickel nitrate is 0.1 mol / L, and the concentration of the ferric nitrate is 0.02 mol / L;

[0077] (2) The monolithic catalyst precursor obtained in step (1) is washed with deionized water, and calcined at 800° C. for 5 h to obtain the foam metal-supported nickel ferrite monolithic catalyst.

[0078] Example 4

[0079] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst, and the preparation method of the foam metal supported nickel ferrite monolithic catalyst comprises the following steps:

[0080] (1) using a nickel foam sheet as a cathode, the first solution as an electrodeposition solution, a platinum sheet as a counter electrode, and a saturated calomel electrode as a reference electrode, performing electrodeposition for 2.5 min at a potential of -1.0 V and 30° C. to obtain a monolithic catalyst precursor;

[0081] The metal foam is pretreated, specifically, the metal foam is sequentially cleaned with hydrochloric acid for 40 seconds, anhydrous ethanol for 12 minutes, acetone for 12 minutes, and deionized water; the concentration of hydrochloric acid in the hydrochloric acid cleaning is 2 mol / L;

[0082] The preparation method of the electrodeposition solution is as follows: mixing the active component solution and 1-ethyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt in a mass ratio of 1:3, stirring and mixing evenly to obtain the electrodeposition solution;

[0083] The active component solution contains nickel nitrate and ferric nitrate, wherein the concentration of the nickel nitrate is 0.1 mol / L, and the concentration of the ferric nitrate is 0.025 mol / L;

[0084] (2) The monolithic catalyst precursor obtained in step (1) is washed with deionized water, and calcined at 650° C. for 3.5 hours to obtain the foam metal-supported nickel ferrite monolithic catalyst.

[0085] Example 5

[0086] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst. The preparation method of the foam metal supported nickel ferrite monolithic catalyst is different from that of Example 1 only in that:

[0087] In this embodiment, the pretreatment process of the metal foam described in step (1) is omitted.

[0088] Example 6

[0089] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst. The preparation method of the foam metal supported nickel ferrite monolithic catalyst is different from that of Example 1 only in that:

[0090] In this embodiment, the mass ratio of the active component solution to the ionic liquid in step (1) is changed to 1:1.

[0091] Example 7

[0092] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst. The preparation method of the foam metal supported nickel ferrite monolithic catalyst is different from that of Example 1 only in that:

[0093] In this embodiment, the mass ratio of the active component solution to the ionic liquid in step (1) is changed to 1:4.

[0094] Example 8

[0095] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst. The preparation method of the foam metal supported nickel ferrite monolithic catalyst is different from that of Example 1 only in that:

[0096] In this example, the concentration of ferric nitrate in the active component solution in step (1) is changed to 0.05 mol / L.

[0097] Example 9

[0098] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst. The preparation method of the foam metal supported nickel ferrite monolithic catalyst is different from that of Example 1 only in that:

[0099] In this example, the concentration of ferric nitrate in the active component solution in step (1) is changed to 0.01 mol / L.

[0100] Example 10

[0101] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst. The preparation method of the foam metal supported nickel ferrite monolithic catalyst is different from that of Example 1 only in that:

[0102] In this embodiment, the calcination temperature in step (2) is changed to 450°C.

[0103] Embodiment 11

[0104] This embodiment provides a foam metal supported nickel ferrite monolithic catalyst. The preparation method of the foam metal supported nickel ferrite monolithic catalyst is different from that of Example 1 only in that:

[0105] In this embodiment, the calcination temperature in step (2) is changed to 850°C.

[0106] Comparative Example 1

[0107] This comparative example provides a monolithic catalyst, and the preparation method of the monolithic catalyst differs from that of Example 1 only in that:

[0108] In this comparative example, the concentration of ferric nitrate in the active component solution in step (1) was changed to 0 mol / L.

[0109] Comparative Example 2

[0110] This comparative example provides a monolithic catalyst, and the preparation method of the monolithic catalyst differs from that of Example 1 only in that:

[0111] In this comparative example, the concentration of nickel nitrate in the active component solution in step (1) was changed to 0 mol / L.

[0112] Comparative Example 3

[0113] This comparative example provides a monolithic catalyst, and the preparation method of the monolithic catalyst differs from that of Example 1 only in that:

[0114] In this comparative example, the ionic liquid in the electrodeposition solution was omitted.

[0115] Comparative Example 4

[0116] This comparative example provides a monolithic catalyst, and the preparation method of the monolithic catalyst comprises the following steps:

[0117] (1) adding nickel nitrate and iron nitrate to deionized water and mixing them evenly to obtain an active component solution; then adding the solution dropwise to a sodium carbonate solution, filtering and rinsing to obtain a precipitate;

[0118] Wherein, the concentration of nickel nitrate in the active component solution is 0.1 mol / L, and the concentration of iron nitrate is 0.03 mol / L;

[0119] (2) calcining the precipitate of step (1) at 700° C. for 4 h to obtain the NiFe2O4 powder monolithic catalyst.

[0120] Application Examples

[0121] The catalysts provided in Examples 1-11 and Comparative Examples 1-4 were used to produce hydrogen by cracking methane.

[0122] The methane cracking hydrogen production process is carried out in a fixed bed reactor. The reaction pressure is normal pressure, the reaction temperature is 600° C., the raw material is 20% CH4 / Ar mixed gas, and the inlet flow rate is 25 ml / min.

[0123] Table 1

[0124]

[0125]

[0126] In summary, the present invention uses NiFe2O4 inverse spinel structure rich in intrinsic defects as an active ingredient and a high specific surface area and porous foam metal as a carrier, which has high methane catalytic activity and stability. In addition, the foam metal-supported nickel ferrite monolithic catalyst is prepared by an in-situ electrodeposition method, and the entire electrodeposition process takes only a short time, simplifies the preparation process and avoids the waste of raw materials.

[0127] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a foam metal supported nickel ferrite monolithic catalyst, characterized in that: The preparation method is as follows: (1) using metal foam as a cathode and a first solution as an electrodeposition solution to perform electrodeposition to obtain a monolithic catalyst precursor; The preparation method of the electrodeposition solution comprises: mixing an active component solution and an ionic liquid, and stirring and mixing them uniformly to obtain the electrodeposition solution; The mass ratio of the active component solution to the ionic liquid is 1:(1.5-3.5); the active component solution is a mixed solution of nickel salt and iron salt; (2) The monolithic catalyst precursor obtained in step (1) is cleaned and calcined to obtain the foam metal-supported nickel ferrite monolithic catalyst.

2. The preparation method according to claim 1, characterized in that: The metal foam in step (1) includes any one of nickel foam, aluminum foam or copper foam.

3. The preparation method according to claim 1, characterized in that: The pore size of the metal foam in step (1) is 50 to 500 μm.

4. The preparation method according to claim 1, characterized in that: The preparation method also includes a pretreatment process for the metal foam in step (1).

5. The preparation method according to claim 4, characterized in that: The pretreatment process is to sequentially clean the metal foam with hydrochloric acid, anhydrous ethanol, acetone and deionized water.

6. The preparation method according to claim 5, characterized in that: The hydrochloric acid cleaning time is 20 to 50 seconds.

7. The preparation method according to claim 5, characterized in that: The concentration of hydrochloric acid in the hydrochloric acid cleaning is 1.5-2.5 mol / L.

8. The preparation method according to claim 5, characterized in that: The water-ethanol cleaning time is 8 to 15 minutes.

9. The preparation method according to claim 5, characterized in that: The acetone cleaning time is 8 to 15 minutes.

10. The preparation method according to any one of claims 1 to 3, characterized in that: The ionic liquid of step (1) includes any one of 1-ethyl-3-methylimidazole, 1-butyl-3-methylimidazole chloride, 1-hexadecyl-3-methylimidazole chloride, 1-ethyl-3-methylimidazole tetrafluoroborate, 1-butyl-3-methylimidazole tetrafluoroborate, 1-ethyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide, 1-butyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide or 1-butyl-3-methylimidazole hexafluoroborate, or a combination of at least two thereof.

11. The preparation method according to claim 1, characterized in that: The nickel salt includes nickel nitrate.

12. The preparation method according to claim 1, characterized in that: The iron salt includes ferric nitrate.

13. The preparation method according to claim 1, characterized in that: The concentration ratio of nickel salt to iron salt in the active component solution is 1:(0.1-0.4).

14. The preparation method according to claim 1, characterized in that: The deposition potential of the electrodeposition in step (1) is -0.5 to -1.5V.

15. The preparation method according to claim 1, characterized in that: The deposition time of the electrodeposition in step (1) is 1 to 3 minutes.

16. The preparation method according to claim 1, characterized in that: The electrodeposition temperature in step (1) is 20 to 60°C.

17. The preparation method according to claim 1, characterized in that: The counter electrode in the electrodeposition of step (1) is a platinum sheet, and the reference electrode is a saturated calomel electrode.

18. The preparation method according to claim 1, characterized in that: The cleaning in step (2) includes rinsing the monolithic catalyst precursor with deionized water.

19. The preparation method according to claim 1, characterized in that: The calcination temperature in step (2) is 500-800°C.

20. The preparation method according to claim 1, characterized in that: The calcination time in step (2) is 3 to 5 hours.

21. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) using metal foam as a cathode, the first solution as an electrodeposition solution, a platinum sheet as a counter electrode, and a saturated calomel electrode as a reference electrode, performing electrodeposition at a potential of -0.5 to -1.5 V and a temperature of 20 to 60° C. for 1 to 3 minutes to obtain a monolithic catalyst precursor; The metal foam is pretreated, specifically, the metal foam is sequentially washed with hydrochloric acid for 20 to 50 seconds, washed with anhydrous ethanol for 8 to 15 minutes, washed with acetone for 8 to 15 minutes, and washed with deionized water; the concentration of hydrochloric acid in the hydrochloric acid washing is 1.5 to 2.5 mol / L; The preparation method of the electrodeposition solution is: mixing the active component solution and the ionic liquid in a mass ratio of 1: (1.5-3.5), stirring and mixing to obtain the electrodeposition solution; The active component solution contains iron nitrate and nickel nitrate, and the concentration ratio of nickel nitrate to iron nitrate in the active component solution is 1:(0.1-0.4); (2) The monolithic catalyst precursor obtained in step (1) is washed with deionized water, and calcined at 500-800° C. for 3-5 hours to obtain the foam metal-supported nickel ferrite monolithic catalyst.

22. A foam metal supported nickel ferrite monolithic catalyst, characterized in that: The foam metal supported nickel ferrite monolithic catalyst is obtained by the preparation method described in any one of claims 1-21.

23. An application of the foam metal supported nickel ferrite monolithic catalyst as claimed in claim 22, characterized in that: The foam metal-supported nickel ferrite monolithic catalyst is used for methane cracking to produce hydrogen.

24. The use according to claim 23, characterized in that The methane cracking and hydrogen production is carried out in a fixed bed reactor.

25. The use according to claim 23, characterized in that The temperature in the methane cracking hydrogen production is 500-800°C.

26. The use according to claim 23, characterized in that The raw material for the methane cracking hydrogen production is CH4 / Ar mixed gas.

27. The use according to claim 23, characterized in that The flow rate of the raw material in the methane cracking hydrogen production is 20-30 mL / min.