A method for preparing glass microtube modified with Pebax1657 polymer
By chemically treating Pebax1657 polymer with carbon nanotubes or cellulose nanocrystals in glass microtubes, the problem of rupture of glass microtubes when storing and transporting hydrogen is solved, improving its resistance to shear stress and stability, ensuring Improve hydrogen storage performance and safety.
Patent Information
- Application Number
- CN202310295027.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Existing glass microtubes are prone to breakage and leakage when storing and transporting hydrogen, resulting in reduced hydrogen storage performance and potential safety hazards.
Through chemical treatment, Pebax1657 polymer and carbon nanotubes or cellulose nanocrystals are used as auxiliary agents to modify the glass microtubes to form Pebax1657 polymer-modified glass microtubes to enhance their resistance to shear stress and stability.
This method improves the shear stress resistance of the glass microtubes, reduces the risk of breakage, enhances hydrogen storage performance and safety, and has the potential for simple operation and large-scale production.
Smart Images

Figure CN116425433B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen storage, and in particular to a method for preparing a glass microtube modified with a Pebax1657 polymer. Background Art
[0002] As a gas with extremely low density, hydrogen has always been a difficult problem in the field of hydrogen preparation in terms of storage and transportation. Commonly used hydrogen storage tanks are large in size, heavy in weight, and high in cost. They are also prone to hydrogen embrittlement, posing a safety hazard. Glass microtubes are an emerging hydrogen storage material with the advantages of small size, light weight, and low cost. However, defects are prone to occur during their preparation, and they are also prone to breakage during winding, use, and transportation, resulting in a decrease in the overall hydrogen storage performance and potential safety issues. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a glass microtube modified with a Pebax1657 polymer, so as to solve the technical problem in the prior art that when storing and transporting hydrogen through glass microtubes, cracks and leakages are prone to occur, which reduces performance or causes safety hazards.
[0004] The present invention provides a method for preparing a glass microtube modified with a Pebax1657 polymer, wherein the glass microtube is treated with a resin by a chemical treatment method, and the method comprises the following steps:
[0005] Sp1: Weigh Pebax1657 polymer and dissolve it in a mixed solution of ethanol and water, stir it thoroughly and heat it;
[0006] Sp2: Weigh auxiliary carbon nanotubes or cellulose nanocrystals and add them to the above solution, and stir them thoroughly;
[0007] Sp3: Immerse the glass microtube completely in the above mixed solution for 10-60 seconds.
[0008] Furthermore, the mixed solution of ethanol and water is one or more of 50:50, 60:40, 70:30, 80:20, and 90:10.
[0009] Furthermore, in Sp1, the auxiliary agent is weighed in 1-5 parts by mass, and the mixed solution of ethanol and water is weighed in 20-50 parts by mass, and the mixture is fully stirred for 2-6 hours, and the heating temperature is 60-90°C.
[0010] Furthermore, in Sp1, the amount of the mixed solution of ethanol and water added is 25-30 parts by mass, and the solution is fully stirred for 2-3 hours.
[0011] Furthermore, in Sp1, the Pebax1657 polymer is weighed in an amount of 1-15 parts by mass, and the solution is fully stirred for 2-6 hours.
[0012] Furthermore, in Sp1, 5-10 parts by mass of the Pebax1657 polymer are weighed, and the solution is fully stirred for 2-4 hours.
[0013] Furthermore, in Sp3, the glass microtube is immersed in the mixed solution for 30-40 seconds.
[0014] Compared with the prior art, the beneficial effects of the present invention are:
[0015] When using glass microtubes to store and transport hydrogen, the defects in the microtubes or the damage caused during the process will affect the overall hydrogen storage performance and safety. Therefore, we designed a glass microtube modified with Pebax1657 polymer, and prepared the glass microtube modified with Pebax1657 polymer by adding auxiliary agents (i.e. carbon nanotubes or cellulose nanocrystals) during the preparation process. This preparation method is simple, easy to operate, and has the potential to achieve large-scale production. In the laboratory preparation process, it can well preserve the morphology of the glass microtube and improve its shear stress resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 A flow chart of the glass microtube chemical treatment method of the present invention;
[0018] Figure 2 This is a scanning electron microscope image of a glass microtube of Example 2 of the present invention;
[0019] Figure 3 This is a schematic diagram of the shear stress of the glass microtube obtained in Example 2 of the present invention;
[0020] Figure 4 This is a scanning electron microscope image of a glass microtube of Example 3 of the present invention;
[0021] Figure 5 This is a schematic diagram of the shear stress of the glass microtube obtained in Example 3 of the present invention;
[0022] Figure 6 This is a scanning electron microscope image of a glass microtube of Example 4 of the present invention;
[0023] Figure 7This is a schematic diagram of the shear stress of the glass microtube obtained in Example 4 of the present invention;
[0024] Figure 8 This is a scanning electron microscope image of a glass microtube of Example 5 of the present invention;
[0025] Fig. 9 This is a schematic diagram of the shear stress of the glass microtube obtained in Example 5 of the present invention;
[0026] Fig.10 This is a scanning electron microscope image of Example 6 of the present invention through a glass microtube;
[0027] Fig.11 This is a schematic diagram of the shear stress resistance of the glass microtube obtained in Example 6 of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0029] The components of the embodiments of the present invention generally described and shown in the drawings herein may be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention.
[0030] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] Combine the following Figure 1 As shown, an embodiment of the present invention provides a method for preparing a glass microtube modified with a Pebax1657 polymer, wherein the glass microtube is treated with a resin by a chemical treatment method, and the method comprises the following steps:
[0033] Sp1: Weigh Pebax1657 polymer into a mixed solution of ethanol and water, stir thoroughly and heat;
[0034] Sp2: weigh auxiliary carbon nanotubes or cellulose nanocrystals into the above solution and stir thoroughly;
[0035] Sp3: Immerse the glass microtube completely in the above mixed solution for 10-60 seconds.
[0036] We designed a method to modify glass microtubes by blending Pebax1657 polymer and auxiliary agents (carbon nanotubes or cellulose nanocrystals). Glass microtubes modified with Pebax1657 polymer were prepared by wrapping Pebax1657 polymer and auxiliary agents (carbon nanotubes or cellulose nanocrystals) on the surface of glass microtubes. This preparation method is simple, easy to operate, and has the potential for large-scale production, which is conducive to further large-scale production. During the experiment, the hollow structure of the glass microtubes was well maintained, which improves the structural stability without affecting the hydrogen storage performance.
[0037] In this embodiment, the mixed solution of ethanol and water is one or more of 50:50, 60:40, 70:30, 80:20, and 90:10.
[0038] In another embodiment, the auxiliary agent is weighed in 1-5 parts by mass, the mixed solution of ethanol and water is weighed in 20-50 parts by mass, and is fully stirred for 2-6 hours, the heating temperature is 60-90°C, and the preferred stirring time is 2-4 hours; the Pebax1657 polymer is weighed in 1-15 parts by mass, and the preferred addition amount is 5-10 parts by mass, and the solution is fully stirred for 2-6 hours, and the preferred stirring time is 2-4 hours; and the glass microtube is preferably immersed in the mixed solution for 30-40 seconds.
[0039] Embodiment 2:
[0040] This embodiment provides a method for preparing a glass microtube, which is carried out according to the following steps:
[0041] Weigh 1 g of Pebax1657 polymer and dissolve it in 50 mL of a mixed solution of ethanol and water (60:40), heat it to 60°C, and stir it for 2 h. After it is dissolved, add 0.1 g of carbon nanotubes and continue stirring for 1 h.
[0042] The scanning electron microscope image of the Pebax1657 polymer modified glass microtube material obtained in this example is shown in FIG. Figure 2 shown. Figure 3 The mechanical properties of the samples were tested, and each sample was tested three times to take the average value. The maximum bearing stress was 5.508MPa.
[0043] Embodiment 3:
[0044] This embodiment provides a method for preparing a glass microtube, which is carried out according to the following steps:
[0045] Weigh 1 g of Pebax1657 polymer and dissolve it in 50 mL of ethanol and water (70:30), heat it to 70°C, and stir it for 2 h. After it is dissolved, add 0.2 g of carbon nanotubes and continue stirring for 1 h.
[0046] The scanning electron microscope image of the Pebax1657 polymer modified glass microtube material obtained in this example is shown in FIG. Figure 4 shown. Figure 5 The mechanical properties of the samples were tested, and each sample was tested three times to take the average value. The maximum bearing stress was 5.851MPa.
[0047] Embodiment 4:
[0048] This embodiment provides a method for preparing a glass microtube, which is carried out according to the following steps:
[0049] Weigh 1 g of Pebax1657 polymer and dissolve it in 50 mL of ethanol and water (70:30), heat it to 80°C, and stir it for 2 h. After it is dissolved, add 0.3 g of carbon nanotubes and continue stirring for 1 h.
[0050] The scanning electron microscope image of the Pebax1657 polymer modified glass microtube material obtained in this example is shown in FIG. Figure 6 shown. Figure 7 The mechanical properties of the samples were tested, and each sample was tested three times to take the average value. The maximum bearing stress was 6.014MPa.
[0051] Embodiment 5:
[0052] This embodiment provides a method for preparing a glass microtube, which is carried out according to the following steps:
[0053] Weigh 1 g of Pebax1657 polymer and dissolve it in 50 mL of ethanol and water (70:30), heat it to 70°C, and stir it for 1 hour. After it is dissolved, add 0.1 g of cellulose nanocrystals and continue stirring for 1 hour.
[0054] The scanning electron microscope image of the Pebax1657 polymer modified glass microtube material obtained in this example is shown in FIG. Figure 8 shown. Fig. 9 The mechanical properties of the samples were tested, and each sample was tested three times to take the average value. The maximum bearing stress was 7.332MPa.
[0055] Embodiment 6:
[0056] This embodiment provides a method for preparing a glass microtube, which is carried out according to the following steps:
[0057] Weigh 1 g of Pebax1657 polymer and dissolve it in 50 mL of ethanol and water (70:30), heat it to 60°C, and stir it for 2 h. After it is dissolved, add 0.2 g of cellulose nanocrystals and continue stirring for 1 h.
[0058] The scanning electron microscope image of the Pebax1657 polymer modified glass microtube material obtained in this example is shown in FIG. Fig.10 shown. Fig.11 The mechanical properties of the samples were tested, and each sample was tested three times to take the average value. The maximum bearing stress was 7.415MPa.
[0059] In summary, the glass microtubes modified with Pebax1657 polymer have superior stability under the maximum bearing stress test, and therefore are safer during the hydrogen storage process.
[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a glass microtube modified with a Pebax1657 polymer, characterized in that: The glass microtube is treated with a polymer by chemical treatment, comprising the following steps: Sp1: Weigh Pebax1657 polymer and add it to a mixed solution of ethanol and water, stir thoroughly and heat; Sp2: weigh auxiliary carbon nanotubes or cellulose nanocrystals into the above solution and stir thoroughly; Sp3: Immerse the glass microtube completely in the above mixed solution for 10-60 seconds.
2. The method for preparing a glass microtube modified with Pebax1657 polymer according to claim 1, characterized in that: The mixed solution of ethanol and water is one or more of 50:50, 60:40, 70:30, 80:20, and 90:
10.
3. The method for preparing a glass microtube modified with Pebax1657 polymer according to claim 1, characterized in that: In Sp1, the auxiliary agent is weighed in 1-5 parts by mass, and the mixed solution of ethanol and water is weighed in 20-50 parts by mass, and the mixture is stirred for 2-6 hours at a heating temperature of 60-90°C.
4. The method for preparing a glass microtube modified with a Pebax1657 polymer according to claim 3, characterized in that: In Sp1, the amount of the mixed solution of ethanol and water added is 25-30 parts by mass, and the solution is fully stirred for 2-3 hours.
5. The method for preparing a glass microtube modified with Pebax1657 polymer according to claim 1, characterized in that: In Sp1, the Pebax1657 polymer is weighed in an amount of 1-15 parts by mass, and the solution is fully stirred for 2-6 hours.
6. The method for preparing a glass microtube modified with Pebax1657 polymer according to claim 4, characterized in that: In Sp1, 5-10 parts by mass of the Pebax1657 polymer are weighed, and the solution is fully stirred for 2-4 hours.
7. The method for preparing a glass microtube modified with Pebax1657 polymer according to claim 1, characterized in that: In Sp3, the glass microtube is immersed in the mixed solution for 30-40 seconds.
Citation Information
Patent Citations
Induction method for glass fiber / polypropylene interface transverse crystal structure
CN112624631A
Modified halloysite nanotube / polyether copolyamide mixed matrix membrane and preparation method thereof
CN112791606A
Extruded thin wall polyether block amide membrane tubing and module
GB2606046A
A copolymer and a gas separation membrane using the same
KR102032947B1
Anti-static flame retardant resin composition and methods for manufacture thereof
US20060020060A1