A high-plasticity and high-purity single-phase austenitic stainless steel and preparation method thereof

Through steps such as smelting, remelting, high-temperature diffusion and heat treatment, the problems of high impurity content and component segregation of austenitic stainless steel are solved, and high-purity, high-plasticity single-phase austenitic stainless steel is prepared to meet the high-performance requirements of special fields and Reduced costs.

CN116426833BActive Publication Date: 2024-10-22SICHUAN JIANGYOU LIUHE STEAM TURBINE MATERIAL +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310223906.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-10-22
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

Existing austenitic stainless steel material preparation methods have high impurity content, resulting in insufficient purity of the material and other phases easily forming during the preparation process, making it unable to meet the high plasticity requirements of special fields.

Method used

Six steps of smelting, remelting, high-temperature diffusion, forging, hot forging and heat treatment are adopted to limit the proportion of specific raw materials. 80 hours of high-temperature diffusion eliminates component segregation, ensuring that the steel only contains the γ austenite phase and reducing non-metallic inclusions. material to improve the uniformity and plasticity of the material.

Benefits of technology

High-purity, high-plasticity single-phase austenitic stainless steel is prepared, which has excellent plasticity, heat resistance and hot processing properties, meets the requirements of use in special fields, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116426833B_ABST
    Figure CN116426833B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-plasticity and high-purity single-phase austenitic stainless steel and a preparation method thereof, and relates to the technical field of special stainless steel preparation. The present invention limits a specific raw material ratio and adopts a processing technology including six steps of smelting, remelting, high-temperature diffusion, forging blanking, hot forging, and heat treatment, so that the austenitic stainless steel prepared contains only γ austenite phase. Among them, the non-metallic inclusions are: Class A fine system 0 level, Class B fine system 0 level, Class C fine system less than 0 level, Class D fine 1.0 level, DS less than 0 level, the sum of the above five categories is 1.0 level, and the sum of the four categories of A, B, C, and D coarse systems is 0 level. The austenitic stainless steel prepared by the present invention has excellent plasticity, heat resistance and hot workability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of special stainless steel preparation, and in particular to a high-plasticity and high-purity single-phase austenitic stainless steel and a preparation method thereof. Background Art

[0002] Austenitic single-phase stainless steel is a stainless steel with a stable austenitic structure at room temperature. Austenitic single-phase stainless steel has excellent plasticity and is widely used in special fields such as aerospace, nuclear industry, and weapons and equipment. With the development of science and technology, special fields have higher and higher requirements for alloy quality. New technologies, new processes, and new equipment are used to improve the quality and performance of special austenitic stainless steel, which greatly improves the cleanliness, uniformity, grain refinement, and size of the material.

[0003] However, the impurity content of the material produced by the current austenitic stainless steel material preparation method is relatively high, resulting in insufficient purity of the austenitic stainless steel. Or other phases are formed during the preparation process, resulting in the plasticity of the austenitic stainless steel failing to meet the requirements of service conditions in special fields.

[0004] Therefore, developing a new process suitable for single-phase austenitic stainless steel to solve the problem of impurities and the formation of new phases in austenitic stainless steel and to obtain excellent plasticity is an urgent problem to be solved for large-scale application of high-purity austenitic stainless steel in special fields. Those skilled in the art have also made many attempts to this end. For example, in the patent application document with publication number CN114686781B, an austenitic stainless steel and its preparation and processing method are proposed. The invention obtains pure austenitic stainless steel through component design and process optimization, and the S and Cu content of the obtained austenitic stainless steel is controlled, the grain size is refined, and the level of four types of inclusions is controlled. However, in terms of its processing flow, an yttrium oxide coating is applied to the surface of the intermediate ingot material, and the oxygen element is further introduced to increase the oxygen content in the austenitic stainless steel. In the patent application document with publication number CN111876653B, a method for preparing pure austenitic stainless steel is proposed. The invention adds lanthanum-cerium rare earth alloy and metal calcium before steel casting. Rare earth modification inclusions can indeed purify the alloy matrix, form high melting point fine particles, refine the structure, and reduce segregation. Excessive addition of rare earth alloy will deteriorate the performance of the material. In addition, the price of rare earth alloy is relatively high, which greatly increases the cost in large-scale production.

[0005] Austenitic stainless steel refers to stainless steel whose alloy structure is single-phase austenite at room temperature. Austenitic stainless steel has better room temperature performance, corrosion resistance and plastic forming performance than ferrite. Austenite is a high-temperature phase. To completely stabilize austenite to room temperature, higher requirements are required for alloy smelting and material processing. Although the above-mentioned prior art can produce pure austenitic stainless steel, rare earth oxides or rare earth elements are introduced therein. The addition of rare earth oxides will introduce oxygen elements into the steel to increase the oxygen content of austenitic stainless steel, and rare earth alloys will degenerate and purify the austenitic stainless steel matrix. However, excessive addition of rare earth alloys will deteriorate the organization and comprehensive properties of the material. At the same time, the price of rare earth alloys is high, which will increase costs in production. Summary of the invention

[0006] In view of the above problems in the prior art, the present invention provides a high-plasticity and high-purity single-phase austenitic stainless steel and a preparation method thereof, which can produce high-plasticity and high-purity single-phase austenitic stainless steel, improve the plasticity and corrosion resistance of the steel by grain refinement and reduction of segregation, and at the same time, the obtained steel contains only austenite γ phase and has a low impurity content.

[0007] The technical solution adopted by the present invention is as follows:

[0008] The invention provides a high-plasticity and high-purity single-phase austenitic stainless steel. The austenitic stainless steel is composed of the following components in percentage by mass: 1.00-2.00% Mn, 11.50-12.50% Ni, 17.00-18.00% Cr, 2.50-2.70% Mo, 0.05-0.07% N, C≤0.03%, Si≤0.60%, S≤0.003%, P≤0.030%, Cu≤0.10%, V≤0.05%, Al≤0.03%, Co≤0.06%, Sn≤0.005%, As≤0.01%, B≤0.0015%, Se≤0.015%, Pb≤0.001%, Bi≤0.00001%, Sb≤0.002%, Zn≤0.01%, five harmful elements and ≤0.015%, H≤5ppm, O≤30ppm, and the balance is Fe.

[0009] A method for preparing high-plasticity and high-purity single-phase austenitic stainless steel comprises the following steps:

[0010] (1) Smelting: Take the raw materials of the required elements and perform alloy smelting on them. The smelting sequence is as follows: primary smelting in a 20T non-vacuum induction furnace, stainless steel argon oxygen blowing in an AOD furnace, LF ladle refining, and VD furnace refining;

[0011] (2) Remelting: Electroslag remelting in protective atmosphere;

[0012] (3) High temperature diffusion: step-wise heating to 1200-1300°C and keeping temperature for 80h;

[0013] (4) Forging and blanking: forging temperature: 1125±20℃, final forging temperature: 800±20℃, after two passes of upsetting and drawing, finally thrown out for cleaning, the steel ingot is hot cut to remove the head and tail rotten materials;

[0014] (5) Hot forging: first heat to 850±20℃ and keep warm for 2h, heating rate: 70±10℃ / h, then heat to 1180±20℃ and keep warm for 3h, heating rate: 140±10℃ / h. After the insulation, start forging. The press is stretched and unloaded in two passes, and then returned to the furnace to be fired at 1180℃ for 40 to 60 minutes. After being taken out of the furnace, it is rounded to the size of a ruler.

[0015] (6) Heat treatment: charging temperature: 580±20℃, heating rate: 140±10℃ / h, keep at 930℃±10℃ for 100min, then heat to 1050±10℃ and keep for 30min, and finally water cool.

[0016] Preferably, in the 20T non-vacuum induction furnace for primary smelting in step (1), the slag weight ratio is CaO:CaF2=1.2:1, and the tapping conditions are: tapping temperature: 1640±20°C, the ladle is well baked, and the ladle temperature is 820±20°C.

[0017] Preferably, in the AOD furnace for argon oxygen blowing of stainless steel in step (1), 800-1000 kg of lime is added to the furnace bottom during steel treatment, 2.4-2.6 tons of CaO are added during the blowing period, 500-700 kg of J-Si is added during the reduction period, 240-300 kg of aluminum ingots are added, and 200-400 kg of fluorite are added.

[0018] Preferably, in the LF ladle refining in step (1), an appropriate amount of Al wire is fed for deoxidation before entering and exiting the workstation, and an appropriate amount of Si-Ca powder / Al powder is added in small batches for deoxidation during refining, and the casting temperature is controlled at 1530-1570°C.

[0019] Preferably, in step (1), the VD furnace refining has a total evacuation time of 15 minutes, an ultimate vacuum of 123±10Pa, an ultimate vacuum time of 6±1min, and sampling after breaking the vacuum for full analysis and temperature measurement for reference. After sampling, the cover is closed and the C, N, and Cr are adjusted after the sample is returned. The hydrogen is set to less than 4PPM, and the composition is uniformly blown with argon. The temperature is suitable for steelmaking, and the ladle temperature is 1530-1550°C.

[0020] Preferably, the remelting slag in step (2) is 57# or 60# slag + SiO2 + MgO.

[0021] Preferably, the forging equipment in steps (4) and (5) are both 5500T forging presses.

[0022] In summary, compared with the prior art, the present invention has the following advantages and beneficial effects:

[0023] 1. The present invention limits the specific raw material ratio and adopts a processing technology including six steps of smelting, remelting, high temperature diffusion, forging blanking, hot forging and heat treatment to prepare austenitic stainless steel containing only γ-austenite phase. Among them, non-metallic inclusions: Class A fine system 0 level, Class B fine system 0 level, Class C fine system less than 0 level, Class D fine 1.0 level, DS less than 0 level, the sum of the above five categories is 1.0 level, and the sum of the four categories of A, B, C, and D coarse systems is 0 level. Among them, C≤0.03%, S≤0.003%, P≤0.030%, N 0.05~0.07%, the sum of the five harmful elements ≤0.015%, H≤5ppm, O≤30ppm;

[0024] 2. The present invention eliminates component segregation and makes the structure uniform through the combination of high-temperature diffusion + forging + heat treatment. In order to achieve single-phase austenitic stainless steel without component segregation and uniform and pure structure, high-temperature diffusion for up to 80 hours is the most effective way to solve this problem;

[0025] 3. The austenitic stainless steel of the present invention has excellent plasticity, heat resistance and hot workability (ductility and impact toughness). It does not peel during forging after being heated at 1200-1300°C for 80 hours. It has good ductility and plasticity within the temperature range of 800-1200°C, and is easy to achieve high-precision forging. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 XRD spectra of austenitic stainless steel obtained in Examples 1 to 3;

[0027] Figure 2 The optical microscope images of the austenitic stainless steel obtained in Examples 1 to 3;

[0028] Figure 3 The tensile stress-strain curves of the austenitic stainless steel examples obtained in Examples 1 to 3 are shown. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and various embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.

[0030] The elemental compositions of the austenitic stainless steels prepared in the following three embodiments are shown in Table 1:

[0031] Table 1 Element composition table of each embodiment

[0032]

[0033]

[0034] The raw materials containing the elements of the austenitic stainless steel prepared in Table 1 include metallic manganese, ferrosilicon, high chromium, nickel plate, ferromolybdenum, aluminum ingots, and chromium nitride, all of which are commercially available and were subjected to component analysis before use.

[0035] Example 1

[0036] The raw materials corresponding to the elemental composition of Example 1 in Table 1 were used to prepare austenitic stainless steel in the following steps:

[0037] (1) Smelting: Take the raw materials of the required elements and use 20T non-vacuum induction furnace + AOD furnace stainless steel argon oxygen blowing + LF ladle refining + VD furnace refining for smelting. The 20T non-vacuum induction furnace slag material ratio is CaO:CaF2=1.2:1 (wt%), and the steel tapping conditions are: steel tapping temperature 1620℃, good ladle baking, and ladle temperature 800℃. The AOD furnace stainless steel argon oxygen blowing, the furnace bottom is padded with lime 800kg / furnace during steel treatment, the total CaO addition amount during the blowing period is 2.5 tons / furnace, and J-Si 650Kg / furnace, aluminum ingot 240Kg / furnace, and fluorite 200kg / furnace are added during the reduction period. The LF ladle refining, feed a proper amount of Al wire before entering and leaving the station for deoxidation, and add a proper amount of Si-Ca powder in small batches during refining for deoxidation. The casting temperature is controlled at 1530℃.

[0038] (2) Remelting: Electroslag remelting is performed in a protective atmosphere. The slag system uses 57# slag + SiO2 + MgO.

[0039] (3) High temperature diffusion: step-by-step heating to 1200°C and keep warm for 80 hours.

[0040] (4) Forging and blanking: The product obtained in step (3) is forged using a 5500T forging press, with a starting forging temperature of 1105°C and a final forging temperature of 780°C. After two passes of upsetting and drawing, the ingot is finally thrown out for cleaning, and the head and tail rotten materials are hot cut.

[0041] (5) Hot forging: The intermediate billet obtained in step (4) is forged using a 5500T forging press. The temperature is first raised to 830°C and kept for 2 hours at a heating rate of 60°C / h, and then raised to 1160°C and kept for 3 hours at a heating rate of 130°C / h. After the insulation is completed, forging begins. The press is stretched and cut in two passes. The billet is returned to the furnace and fired at 1180°C for 40 minutes. After it is taken out of the furnace, it is rounded to a size of 1.0 mm.

[0042] (6) Heat treatment: charging temperature 560°C, heating rate 130°C / h, keeping at 920°C for 100 min, then heating to 1040°C and keeping for 30 min, cooling by water, the obtained austenitic stainless steel is named 1.

[0043] Example 2

[0044] The raw materials corresponding to the elemental composition of Example 2 in Table 1 were used to prepare austenitic stainless steel in the following steps:

[0045] (1) Smelting: Take the raw materials of the required elements and use 20T non-vacuum induction furnace + AOD furnace stainless steel argon oxygen blowing + LF ladle refining + VD furnace refining for smelting. The 20T non-vacuum induction furnace slag material ratio is CaO:CaF2=1.2:1 (wt%), and the steel tapping conditions are: steel tapping temperature 1640℃, good ladle baking, and ladle temperature 820℃. The AOD furnace stainless steel argon oxygen blowing, the furnace bottom is padded with lime 900kg / furnace during steel treatment, the total CaO addition amount during the blowing period is 2.5 tons / furnace, and J-Si 600Kg / furnace, aluminum ingot 270Kg / furnace, and fluorite 300kg / furnace are added during the reduction period. The LF ladle refining, feed a proper amount of Al wire before entering and leaving the station for deoxidation, and add a proper amount of Si-Ca powder in small batches during refining for deoxidation. The casting temperature is controlled at 1550℃.

[0046] (2) Remelting: Electroslag remelting is performed in a protective atmosphere. The slag system uses 57# slag + SiO2 + MgO.

[0047] (3) High temperature diffusion: step-by-step heating to 1250°C and keep warm for 80 h.

[0048] (4) Forging and blanking: The product obtained in step (3) is forged using a 5500T forging press, with the starting forging temperature being 1125°C and the final forging temperature being 800°C. After two passes of upsetting and drawing, the product is finally thrown out for cleaning, and the head and tail of the steel ingot are hot-cut.

[0049] (5) Hot forging: The intermediate billet obtained in step (4) is forged using a 5500T forging press. The temperature is first raised to 850°C and kept for 2 hours at a heating rate of 70°C / h, and then raised to 1180°C and kept for 3 hours at a heating rate of 140°C / h. After the insulation is completed, forging begins. The press is stretched and cut in two passes. The billet is returned to the furnace and fired at 1180°C for 50 minutes. After it is taken out of the furnace, it is rounded to a size of 1.0 mm.

[0050] (6) Heat treatment: charging temperature 580°C, heating rate 140°C / h, keeping at 930°C for 100 min, then heating to 1050°C and keeping for 30 min, cooling by water, the obtained austenitic stainless steel is named 2.

[0051] Example 3

[0052] The raw materials corresponding to the elemental composition of Example 3 in Table 1 were used to prepare austenitic stainless steel in the following steps:

[0053] (1) Smelting: Take the raw materials of the required elements and use 20T non-vacuum induction furnace + AOD furnace stainless steel argon oxygen blowing + LF ladle refining + VD furnace refining for smelting. The 20T non-vacuum induction furnace slag material ratio is CaO:CaF2=1.2:1 (wt%), and the tapping conditions are: tapping temperature 1660℃, good ladle baking, and ladle temperature 840℃. The AOD furnace stainless steel argon oxygen blowing, the furnace bottom is padded with 1000kg / furnace lime during steel treatment, the total CaO addition during the blowing period is 2.6 tons / furnace, and J-Si 700Kg / furnace, aluminum ingot 300Kg / furnace, and fluorite 400kg / furnace are added during the reduction period. The LF ladle refining, feed a proper amount of Al wire before entering and leaving the station for deoxidation, and add a proper amount of Si-Ca powder in small batches during refining for deoxidation. The casting temperature is controlled at 1570℃.

[0054] (2) Remelting: Electroslag remelting is performed in a protective atmosphere. The slag system uses 60# slag + SiO2 + MgO.

[0055] (3) High temperature diffusion: step-by-step heating to 1300°C and keep warm for 80 hours.

[0056] (4) Forging and blanking: The product obtained in step (3) is forged using a 5500T forging press, with a starting forging temperature of 1145°C and a final forging temperature of 820°C. After two passes of upsetting and drawing, the ingot is finally thrown out for cleaning, and the head and tail rotten materials are hot cut.

[0057] (5) Hot forging: The intermediate billet obtained in step (4) is forged using a 5500T forging press. The temperature is first raised to 870°C and kept for 2 hours at a heating rate of 80°C / h, and then raised to 1200°C and kept for 3 hours at a heating rate of 150°C / h. After the insulation is completed, forging begins. The press is stretched and cut in two passes. The billet is returned to the furnace and fired at 1180°C for 60 minutes. After it is taken out of the furnace, it is rounded to a size of 1.0 mm.

[0058] (6) Heat treatment: charging temperature 600 °C, heating rate 150 °C / h, keeping at 940 °C for 100 min, then heating to 1060 °C and keeping for 30 min, cooling by water, the obtained austenitic stainless steel is named 3.

[0059] Test Example 1

[0060] The inclusion content of the stainless steel obtained in Examples 1 to 3 was measured using the latest national standard. The test results are shown in Table 2.

[0061] Table 2 Example inclusion category and grade table

[0062]

[0063] Note: The values ​​in the table are all inclusion levels

[0064] Test Example 2

[0065] The austenitic stainless steels obtained in Examples 1, 2 and 3 were characterized by X-ray diffraction and optical microscopy for physical and metallographic characteristics. Figure 1 XRD spectrum of austenitic stainless steel. Figure 2 The results show that the austenitic stainless steels obtained in Examples 1, 2 and 3 of the present invention are all single γ-phase austenite.

[0066] Test Example 3

[0067] The heat resistance, hot working performance and plasticity of the austenitic stainless steel obtained in Examples 1, 2 and 3 were tested. Figure 3 The room temperature tensile stress-strain curve of austenitic stainless steel. The results show that austenitic stainless steel does not scale when forged after heating at 1220-1260℃ for 80h. It has good plasticity and ductility in the high temperature range of 800-1200℃ and is easy to forge. The obtained austenitic stainless steel has excellent ductility, impact toughness and plasticity.

[0068] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A high-plasticity and high-purity single-phase austenitic stainless steel, It is characterized in that The austenitic stainless steel is composed of the following components in mass percentage: Mn 1.00-2.00%, Ni 11.50-12.50%, Cr 17.00-18.00%, Mo 2.50-2.70%, N 0.05~0.07%, C≤0.03%, Si≤0.60%, S≤0.003%, P≤0.030%, Cu≤0.10%, V≤0.05%, Al≤0.03%, Co≤0.06%, Sn≤0.005%, As≤0.01%, B≤0.0015%, Se≤0.015%, Pb≤0.001%, Bi≤0.00001%, Sb≤0.002%, Zn≤0.01%, five harmful elements and ≤0.015%, H≤5ppm, O≤30ppm, and the balance is Fe; the obtained austenitic stainless steel is a γ phase, and the preparation process of austenitic stainless steel includes the following steps: (1) Smelting: Take the raw materials of the required elements and perform alloy smelting on them. The smelting sequence is as follows: primary smelting in a 20T non-vacuum induction furnace, stainless steel argon oxygen blowing in an AOD furnace, LF ladle refining, and VD furnace refining; (2) Remelting: Electroslag remelting in protective atmosphere; (3) High temperature diffusion: step-wise heating to 1200-1300°C and keeping temperature for 80 hours; (4) Forging and blanking: forging temperature: 1125±20℃, final forging temperature: 800±20℃, after two passes of upsetting and drawing, finally thrown out for cleaning, the steel ingot is hot cut to remove the head and tail rotten materials; (5) Hot forging: first heat to 850±20℃ and keep warm for 2h, heating rate: 70±10℃ / h, then heat to 1180±20℃ and keep warm for 3h, heating rate: 140±10℃ / h, after the heat preservation, start forging, press to draw and cut the material twice, return to the furnace and burn at 1180℃ for 40-60 minutes, and then round it to the ruler after it comes out of the furnace; (6) Heat treatment: charging temperature: 580±20℃, heating rate: 140±10℃ / h, keep at 930℃±10℃ for 100min, then heat to 1050±10℃ and keep for 30min, and finally water cool.

2. A method for preparing high-plasticity and high-purity single-phase austenitic stainless steel as claimed in claim 1, It is characterized in that The steps include: (1) Smelting: Take the raw materials of the required elements and perform alloy smelting on them. The smelting sequence is as follows: primary smelting in a 20T non-vacuum induction furnace, stainless steel argon oxygen blowing in an AOD furnace, LF ladle refining, and VD furnace refining; (2) Remelting: Electroslag remelting in protective atmosphere; (3) High temperature diffusion: step-wise heating to 1200-1300°C and keeping temperature for 80 hours; (4) Forging and blanking: forging temperature: 1125±20℃, final forging temperature: 800±20℃, after two passes of upsetting and drawing, finally thrown out for cleaning, the steel ingot is hot cut to remove the head and tail rotten materials; (5) Hot forging: first heat to 850±20℃ and keep warm for 2h, heating rate: 70±10℃ / h, then heat to 1180±20℃ and keep warm for 3h, heating rate: 140±10℃ / h, after the heat preservation, start forging, press to draw and cut the material twice, return to the furnace and burn at 1180℃ for 40-60 minutes, and then round it to the ruler after it comes out of the furnace; (6) Heat treatment: charging temperature: 580±20℃, heating rate: 140±10℃ / h, keep at 930℃±10℃ for 100min, then heat to 1050±10℃ and keep for 30min, and finally water cool.

3. The method for preparing high-plasticity and high-purity single-phase austenitic stainless steel according to claim 2, It is characterized in that The 20T non-vacuum induction furnace in step (1) is used for primary smelting, and the weight ratio of slag is CaO:CaF 2 =1.2:1, tapping conditions: tapping temperature: 1640±20℃, ladle baking is good, ladle temperature: 820±20℃.

4. The method for preparing high-plasticity and high-purity single-phase austenitic stainless steel according to claim 2, It is characterized in that In the step (1), the AOD furnace stainless steel argon oxygen blowing is performed, and the furnace bottom is padded with lime 800-1000 kg / furnace during the steel treatment, the total CaO addition amount during the blowing period is 2.4-2.6 tons / furnace, and J-Si 500-700 kg / furnace, aluminum ingot 240-300 kg / furnace, and fluorite 200-400 kg / furnace are added during the reduction period.

5. The method for preparing high-plasticity and high-purity single-phase austenitic stainless steel according to claim 2, It is characterized in that In step (1), the LF ladle is refined, and an appropriate amount of Al wire is fed for deoxidation before entering and leaving the workstation. During the refining, an appropriate amount of Si-Ca powder / Al powder is added in small batches for deoxidation, and the casting temperature is controlled at 1530-1570°C.

6. The method for preparing high-plasticity and high-purity single-phase austenitic stainless steel according to claim 2, It is characterized in that In step (1), the VD furnace refining has a total evacuation time of 15 minutes, an ultimate vacuum of 123±10Pa, and an ultimate vacuum time of 6±1min. After breaking the vacuum, samples are taken for full analysis and temperature measurement for reference. After sampling, the cover is closed and the C, N, and Cr are adjusted after the sample is returned. The hydrogen is set to less than 4PPM, and the composition is uniformly blown with pure argon. The temperature is suitable for steelmaking, and the ladle temperature is 1530-1550°C.

7. The method for preparing high-plasticity and high-purity single-phase austenitic stainless steel according to claim 2, It is characterized in that In step (2), the remelting slag is 57# or 60# slag + SiO 2 +MgO.

8. The method for preparing high-plasticity and high-purity single-phase austenitic stainless steel according to claim 2, It is characterized in that The forging equipment in steps (4) and (5) both adopt a 5500T forging press.